A method for preparing a two-dimensional carbon material and a two-dimensional carbon material prepared thereby
By constructing PVP competitive coordination 3D MOFs materials through solvothermal method and carrying out high-temperature pyrolysis, the problems of low synthesis yield and easy agglomeration of two-dimensional MOFs materials were solved. Two-dimensional metal/carbon materials with plate-like structure and controllable metal particle size were prepared, which improved the catalytic performance.
Patent Information
- Application Number
- CN202311764465.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-21
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-12-21
AI Technical Summary
Existing technologies are difficult to effectively prepare two-dimensional MOF-derived metal/carbon composites. The materials have low synthesis yields and are prone to agglomeration, resulting in a small accessible surface area and affecting catalytic performance.
Three-dimensional MOFs materials with competitive coordination of polyvinylpyrrolidone (PVP) were constructed by a solvothermal method and pyrolyzed at high temperature in an inert atmosphere. Subsequently, metal modification and carbonization were carried out to prepare two-dimensional metal/carbon materials.
The prepared two-dimensional metal/carbon material has a sheet-like structure and controllable metal particle size, which improves mass transfer efficiency and catalytic performance, making it suitable for the catalytic field.
Smart Images

Figure CN118179548B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of porous carbon materials technology, and in particular to a method for preparing two-dimensional carbon materials and the method for obtaining two-dimensional carbon materials at a specific temperature. Background Technology
[0002] Two-dimensional materials are a current research hotspot, and they have many advantages in the fields of catalysis and energy conversion (J. Am. Chem. Soc. 2016, 138(22), 6924-6927; J. Am. Chem. Soc. 2019, 141(10), 4209-4213; Adv. Mater. 2015, 27(47), 7824-7831.): (1) High accessible surface area is conducive to increasing the contact between reactants and catalyst active sites; (2) Short mass transfer distance and wide contact surface, thereby improving the efficiency of mass transfer process; (3) The edge atoms of two-dimensional materials are unsaturated and form dangling bonds, which helps to stabilize reactant intermediates and reduce the activation energy of the reaction.
[0003] Metal-organic frameworks (MOFs) are a class of porous crystalline materials with periodic network structures formed by the self-assembly of transition metal ions and organic ligands. Most MOFs are three-dimensional porous materials with periodic network structures, and their pyrolysis-derived porous carbon materials also possess 3D structures. Due to their high specific surface area and tunable structures, porous materials have attracted widespread attention in the field of catalysis (Nano-Micro Lett. 2021, 13, 156). However, 3D MOF-derived M / C materials typically have a limited exposed surface area, resulting in fewer active sites for catalysis.
[0004] Currently, the preparation of 2D M / C materials by pyrolysis of 2D MOFs has been reported. However, the preparation of 2D MOFs mainly faces problems such as low synthesis yield and the presence of unsaturated coordination bonds on the surface, which tend to stack and agglomerate during subsequent preparation processes (J. Am. Chem. Soc. 2015, 137(42), 13440-13443; Angew. Chem. Int. Edit. 2016, 55(16), 5019-5023.). However, most 2D MOFs are difficult to prepare because they tend to agglomerate and usually exhibit 3D structures. In addition, two-dimensional (2D) MOFs are easily broken during pyrolysis. Therefore, the technology for directly preparing 2D M / C materials from 2D MOFs by thermal exfoliation still needs improvement.
[0005] On the other hand, there are only a few reports on the preparation of 2D M / C composites using 3D MOF materials, and there has been no substantial breakthrough in the synthetic methods (Nano Lett. 2020, 20, 7342-7349, Nature Chem. 2016, 8, 718–724). In summary, the preparation of 2D metal / carbon composites using 3D MOFs as precursors through novel synthetic methods still needs further research. Summary of the Invention
[0006] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for preparing two-dimensional carbon materials.
[0007] To achieve the objectives of this invention, the technical solution adopted is as follows: A method for preparing a two-dimensional carbon material includes the following steps: (1) Dissolve the metal salt, PVP and organic ligand in N,N-dimethylformamide solvent, and dissolve by sonication and stirring to obtain a mixed solution; (2) The mixed solution in step (1) is heated to crystallize, and after cooling, it is filtered, washed, and dried to obtain 3D MOFs material; (3) The 3D MOFs material in step (2) is subjected to high-temperature pyrolysis and exfoliation under an inert atmosphere to obtain 2D M / C material; (4) The 2D M / C material in step (3) is partially oxidized under an oxygen-argon atmosphere to obtain 2D M-MO / C; (5) The 2D M-MO / C material in step (4) is ultrasonically dispersed in deionized water, followed by the addition of a noble metal solution and ultrasonic displacement to obtain the 2D MM2-MO / C material; (6) Place the 2D MM2-MO / C material from step (5) in a tube furnace, introduce CO gas, and heat treat it at high temperature to obtain the 2D M2-MC / C material.
[0008] This invention constructs three-dimensional (3D) MOFs materials with competitive coordination of polyvinylpyrrolidone (PVP) via a solvothermal method. The MOFs materials are then subjected to high-temperature pyrolysis in an inert atmosphere to obtain 2D metal / carbon materials. Subsequent metal modification and reduction treatment of the metal-metal carbide / carbon materials prepare other metal-metal carbide / carbon materials. These 2D metal-metal carbide / carbon materials not only possess a plate-like structure, which shortens the substrate diffusion distance and achieves efficient mass transfer, but also allow for controllable particle size of the metal on the surface, thus improving the catalytic performance. This method is simple to operate and has good versatility, making it a promising candidate for catalysis.
[0009] Preferably, in step (1), the metal salt is anhydrous FeCl3 or anhydrous Cu(AC)2, and the molar concentration of the metal salt in N,N-dimethylformamide solvent is 0.02~0.40 mol / L; the molecular weight of the PVP is greater than 1 million, and the molar concentration of the PVP in N,N-dimethylformamide solvent is 3.8*10 -6 ~1.5*10 -5 The organic ligand is terephthalic acid, and the molar concentration of the organic ligand in N,N-dimethylformamide solvent is 0.02~0.40 mol / L.
[0010] Preferably, in step (1), the time for ultrasonication and stirring to dissolve is 60~120 min.
[0011] Preferably, in step (2), the temperature of the heating crystallization is 120~150℃, and the heating crystallization time is 12~24h.
[0012] Preferably, in step (3), the inert atmosphere is nitrogen or argon; the pyrolysis stripping temperature is 500~1000℃, and the pyrolysis stripping time is 0.5~5h.
[0013] Preferably, in step (4), the oxidation temperature is 400~600℃.
[0014] Preferably, in step (5), the noble metal solution is a Rh(NO3)3 solution.
[0015] Preferably, in the noble metal solution, the loading of Rh is 1~10mg per 100mg of metal-metal oxide / C; the ultrasonic replacement time is 6~12h.
[0016] Preferably, in step (6), the processing temperature is 300~500℃ and the heat treatment time is 3~6h.
[0017] The present invention also provides 2D metal-metal carbide / carbon materials prepared by the above-mentioned method for preparing two-dimensional carbon materials.
[0018] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. This invention constructs three-dimensional (3D) MOFs materials with competitive coordination of polyvinylpyrrolidone (PVP) using a solvothermal method. The MOFs materials are then subjected to high-temperature pyrolysis in an inert atmosphere to obtain 2D metal / carbon materials. Subsequently, the metal / carbon materials are modified with a second metal and carbonized to prepare metal-metal carbide / carbon materials. These 2D metal-metal carbide / carbon materials not only possess a plate-like structure, which shortens the diffusion distance of the substrate and achieves efficient mass transfer, but also allow for controllable particle size of the metal on the surface, which is beneficial to the catalytic performance of the material. This method is simple to operate and has good versatility, showing potential application prospects in catalysis.
[0019] 2. The formation and synthesis mechanism of PVP competitive coordination 3D MOFs prepared by this invention is novel. During the synthesis of 3D Fe-MOF or Cu-MOF, the C=O in PVP competes with the secondary structural units of the M cluster for coordination, resulting in coordination loss, thereby obtaining 3D MOF materials with a large number of defect sites.
[0020] 3. In the process of synthesizing 3D Fe-MOF or Cu-MOF, the present invention constructs defective units, which decompose rapidly during pyrolysis due to their low stability, thereby promoting the exfoliation of the 3D structure and preparing 2D metal / carbon materials. This is beneficial for efficient mass transfer and has potential practical application value.
[0021] 4. The 2D metal / carbon material prepared in this invention is used for the thermocatalytic hydrogenation of CO to produce gasoline products. At 260°C and a reaction pressure of 2 MPa, the production rate of long-chain hydrocarbons can reach 510 mmol g. -1 h -1 . Attached Figure Description
[0022] Figure 1 The X-ray diffraction (XRD) spectra of Fe-MOF(PVP) and Fe-MOF prepared in Example 1 and Comparative Example 1 of this invention are shown. Figure 2 This is a scanning electron microscope (SEM) image of the Fe-MOF(PVP) prepared in Example 1 of the present invention; Figure 3 This is a scanning electron microscope (SEM) image of the 2D Fe / C material prepared in Example 1 of the present invention; Figure 4 This is a scanning electron microscope (SEM) image of the 2D FeRh-Fe2O3 / C material prepared in Example 1 of the present invention; Figure 5 The X-ray diffraction (XRD) pattern of the 2D Rh-Fe5C2 / C material prepared in Example 1 of this invention; Figure 6This is a scanning electron microscope (SEM) image of the 2D Rh-Fe5C2 / C material prepared in Example 1 of the present invention; Figure 7 The attached figure shows the nitrogen adsorption and desorption process of the 2D Rh-Fe5C2 / C material prepared in Example 1 of this invention; Figure 8 This is a transmission electron micrograph (TEM) of the 2D Rh-Fe5C2 / C material prepared in Example 1 of the present invention. Figure 9 The image shows a scanning electron microscope (SEM) image of the 2D Rh-Fe5C2 / C material prepared in Example 2 of this invention. Figure 10 The graph shows the performance of the 2D Rh-Fe5C2 / C material in Example 3 of this invention in catalyzing CO hydrogenation. Detailed Implementation
[0023] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings and embodiments. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. In the following embodiments, unless otherwise specified, the experimental materials and reagents can be obtained commercially. Where specific techniques or conditions are not specified in the embodiments, they can be performed according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0024] Comparative Example 1 This comparative example provides a traditional method for preparing Fe-MOF, including the following steps: Step 1: Take 900 mg FeCl3 (0.5 mmol) and 222 mg terephthalic acid (0.5 mmol), and dissolve them in N,N-dimethylformamide solvent (40 mL) by sonication and stirring to obtain a mixed solution; Step 2: Heat the mixed solution from Step 1 to crystallize at a temperature of 145℃ for 12 hours; after cooling, centrifuge, wash, and dry to obtain Fe-MOF. Step 3: Pyrolyze the Fe-MOF obtained in Step 2 under an inert atmosphere, heat to 600℃ and hold for 5 hours. After cooling, 3D Fe / C is obtained. Step 4: Partially oxidize the 3D Fe / C obtained in Step 3 under an oxygen-argon atmosphere, heat to 500℃ and hold for 1 hour. After cooling, 3D Fe-Fe2O3 / C is obtained. Step 5: Disperse the 3D Fe-Fe2O3 / C obtained in Step 4 in deionized water by ultrasonication, then add a small amount of Rh(NO3)3 solution and ultrasonically replace for 12 hours to obtain 3D FeRh-Fe2O3 / C. Step 6: Place the 3D FeRh-Fe2O3 / C obtained in Step 5 into a tube furnace, introduce CO gas, and heat treat at 350℃ for 2 hours. After cooling, 3D Rh-Fe5C2 / C is obtained.
[0025] Example 1 This embodiment provides a method for preparing 3D Fe-MOFs that undergo thermal exfoliation and PVP competitive coordination to transform into 2D Fe / carbon materials, including the following steps: (1) Dissolve FeCl3 (0.4 mmol), terephthalic acid (0.6 mmol) and PVP (molecular weight 1.3 million) in N,N-dimethylformamide solvent (40 mL), and sonicate and stir for 30 min to obtain a mixed solution; (2) The mixed solution obtained in step (1) was transferred to a reaction vessel lined with polytetrafluoroethylene, heated to 145°C and maintained for 12 h. After cooling to room temperature, it was filtered, washed three times with N,N-dimethylformamide, and then washed twice with anhydrous ethanol. It was dried at 60°C for 12 h to obtain 3D Fe-MOFs with PVP competitive coordination, denoted as Fe-MOF(PVP). (3) Pyrolyze the Fe-MOF(PVP) in step (2) under an inert atmosphere, heat it to 600℃ and keep it at that temperature for 5 hours. After cooling, 2D Fe / C is obtained. (4) The 2D Fe / C in step (3) is partially oxidized in an oxygen-argon atmosphere, heated to 500℃ and kept at that temperature for 1 hour. After cooling, 2D Fe-Fe2O3 / C is obtained. (5) Disperse the 2D Fe-Fe2O3 / C from step (4) in deionized water by ultrasonication, then add a small amount of Rh(NO3)3 solution and ultrasonically replace for 12 h to obtain 2D FeRh-Fe2O3 / C; (6) Place the 2D FeRh-Fe2O3 / C from step (5) in a tube furnace, introduce CO gas, and heat treat it at 350°C for 2 hours. After cooling, 2D Rh-Fe5C2 / C is obtained.
[0026] Figure 1 The X-ray diffraction (XRD) spectra of Fe-MOF(PVP) and Fe-MOF prepared in Example 1 and Comparative Example 1 are shown below. Figure 1The results show that both Fe-MOF(PVP) and Fe-MOF have good crystallinity and strong crystal diffraction for X-rays. The diffraction peak positions of the two are consistent, indicating that the competitive coordination between PVP and terephthalic acid does not destroy the topological structure of Fe-MOF(PVP).
[0027] Figure 2 The image shown is a scanning electron microscope (SEM) image of the Fe-MOF(PVP) prepared in Example 1. Figure 2 The results show that the Fe-MOF(PVP) prepared in Example 1 has a 3D solid structure and surface cracks.
[0028] Figure 3 The image shown is a scanning electron microscope (SEM) image of the 2D Fe / C prepared in Example 1, based on... Figure 3 The results show that the 2D Fe / C material prepared in Example 1 has a 2D sheet-like structure.
[0029] Figure 4 The image shown is a scanning electron microscope (SEM) image of the 2D FeRh-Fe2O3 / C prepared in Example 1. Figure 4 The results show that the 2D FeRh-Fe2O3 / C material prepared in Example 1 has a 2D sheet-like structure.
[0030] Figure 5 The image shows the X-ray diffraction pattern of 2D Rh-Fe5C2 / C prepared in Example 1. Figure 5 The results show that the diffraction peaks of the material prepared in Example 1 belong to Fe5C2, and because the content of Rh is relatively low, it cannot be observed in the X-ray diffraction pattern.
[0031] Figure 6 Scanning electron microscope (SEM) images of the 2D Rh-Fe5C2 / C prepared in Example 1, according to... Figure 6 The results show that the 2D Rh-Fe5C2 / C material prepared in Example 1 has a 2D sheet-like structure.
[0032] Figure 7 The nitrogen adsorption-desorption diagram of the 2D Rh-Fe5C2 / C prepared in Example 1 is shown in Figure 1. Figure 7 The results show that the 2D Rh-Fe5C2 / C material prepared in Example 1 has micropores and mesopores. The porous structure of the material is conducive to the effective contact between the reactants and the exposed active sites. Figure 8 TEM images of the 2D Rh-Fe5C2 / C material prepared in Comparative Example 1, based on Figure 8The results show that Fe5C2 nanoparticles are uniformly dispersed on the 2D material. Compared with the 3DRh-Fe5C2 / C material prepared by the method in Comparative Example 1, the 2D Rh-Fe5C2 / C material prepared in Example 1 has advantages such as high utilization rate of active sites Rh and Fe5C2 and low mass transfer resistance.
[0033] Example 2 This embodiment provides a method for preparing 3D Cu-MOFs that undergo thermal exfoliation and PVP competitive coordination to transform into 2D Cu / carbon materials, including the following steps: (1) Cu(Ac)2 (0.4 mmol), terephthalic acid (0.6 mmol) and PVP (molecular weight 1.3 million) were dissolved in N,N-dimethylformamide solvent (40 mL), and the mixture was sonicated and stirred for 30 min to obtain a mixed solution. (2) The mixed solution obtained in step (1) was transferred to a reaction vessel lined with polytetrafluoroethylene, heated to 145°C and maintained for 12 h. After cooling to room temperature, it was filtered, washed three times with N,N-dimethylformamide, and then washed twice with anhydrous ethanol. It was dried at 60°C for 12 h to obtain 3D Fe-MOFs with PVP competitive coordination, denoted as Cu-MOF(PVP). (3) The Cu-MOF(PVP) in step (2) is pyrolyzed in an inert atmosphere, heated to 600℃ and kept at that temperature for 5h. After cooling, 2D Cu / C is obtained.
[0034] Figure 9 The image shown is a scanning electron microscope (SEM) image of the hollow 2D Cu / C prepared in Example 2. Figure 9 The results show that Cu / C has a 2D lamellar structure.
[0035] Example 3 This embodiment tests the catalytic performance of the 2D Rh-Fe5C2 / C prepared in Example 1, using the following method: 50 mg of 2D Rh-Fe5C2 / C prepared in Example 1 was placed in a fixed bed, and a mixture of CO and hydrogen gas (V) was introduced at 2 MPa. Ar :V CO :V H2 The mixture (4:32:64) was introduced into a fixed bed at a reaction temperature of 260℃ and a flow rate of 40 mL / min. -1 The result of the reaction is as follows: Figure 10 As shown, according to Figure 10 The results show that, under these reaction conditions, the production rate of long-chain hydrocarbons can reach 510 mmol g. -1 h -1 .
[0036] This invention constructs three-dimensional (3D) MOFs materials with competitive coordination of polyvinylpyrrolidone (PVP) via a solvothermal method. The MOFs materials are then subjected to high-temperature pyrolysis in an inert atmosphere to obtain 2D metal / carbon materials. Subsequently, the metal-metal carbide / carbon materials are modified with a second metal and subjected to carbonization to prepare other metal-metal carbide / carbon materials. These 2D metal-metal carbide / carbon materials not only possess a plate-like structure, which shortens the diffusion distance of the substrate and achieves efficient mass transfer, but also have controllable metal particle size on the surface, which is beneficial to the catalytic performance of the material. This method is simple to operate and has good versatility, showing potential application prospects in catalysis. The embodiments disclosed in this invention are preferred embodiments, but are not limited thereto. Those skilled in the art can easily understand the spirit of this invention based on the above embodiments and make different extensions and variations, but as long as they do not depart from the spirit of this invention, they are all within the protection scope of this invention.
Claims
1. A method for preparing a two-dimensional carbon material, characterized in that, Includes the following steps: (1) Dissolve the metal salt, PVP and organic ligand in N,N-dimethylformamide solvent, and dissolve by sonication and stirring to obtain a mixed solution; (2) The mixed solution in step (1) is heated to crystallize, and after cooling, it is filtered, washed, and dried to obtain 3D MOFs material; (3) The 3D MOFs material in step (2) is subjected to high-temperature pyrolysis and exfoliation under an inert atmosphere to obtain 2D M / C material; (4) The 2D M / C material in step (3) is partially oxidized under an oxygen-argon atmosphere to obtain 2D M-MO / C; (5) The 2D M-MO / C material in step (4) is ultrasonically dispersed in deionized water, followed by the addition of a noble metal solution and ultrasonic displacement to obtain the 2D MM2-MO / C material; (6) Place the 2D MM2-MO / C material from step (5) in a tube furnace, introduce CO gas, and heat treat it at high temperature to obtain the 2D M2-MC / C material.
2. The method for preparing two-dimensional carbon materials according to claim 1, characterized in that: Step (1): The metal salt is anhydrous FeCl3 or anhydrous Cu(AC)2, and the molar concentration of the metal salt in N,N-dimethylformamide solvent is 0.02~0.40 mol / L; the molecular weight of the PVP is greater than 1 million, and the molar concentration of the PVP in N,N-dimethylformamide solvent is 3.8 × 10⁻⁶. -6 ~1.5×10 -5 The organic ligand is terephthalic acid, and the molar concentration of the organic ligand in N,N-dimethylformamide solvent is 0.02~0.40 mol / L.
3. The method for preparing two-dimensional carbon materials according to claim 1, characterized in that: In step (1), the time for ultrasonication and stirring to dissolve is 60~120 min.
4. The method for preparing two-dimensional carbon materials according to claim 1, characterized in that: In step (2), the temperature for heating and crystallization is 120~150℃, and the time for heating and crystallization is 12~24h.
5. The method for preparing two-dimensional carbon materials according to claim 1, characterized in that: In step (3), the inert atmosphere is nitrogen or argon; the pyrolysis stripping temperature is 500~1000℃, and the pyrolysis stripping time is 0.5~5h.
6. The method for preparing two-dimensional carbon materials according to claim 1, characterized in that: In step (4), the temperature of the partial oxidation is 400~600℃.
7. The method for preparing two-dimensional carbon materials according to claim 1, characterized in that: In step (5), the noble metal solution is a Rh(NO3)3 solution.
8. The method for preparing two-dimensional carbon materials according to claim 7, characterized in that: In the noble metal solution, the loading of Rh is 1~10mg per 100mg M-MO / C; the ultrasonic replacement time is 6~12h.
9. The method for preparing two-dimensional carbon materials according to claim 1, characterized in that: In step (6), the processing temperature is 300~500℃ and the heat treatment time is 3~6h.
10. A 2D M2-MC / C prepared by a method for preparing two-dimensional carbon materials as described in any one of claims 1-9.
Citation Information
Patent Citations
Preparation method of bimetallic carbon nano composite electrocatalytic material containing Co and Ru
CN108754531A
Preparation method of two-dimensional MOF derivative carbide
CN108946732A