A method for brazing SiC using ZrCu solder f Methods for using SiC composites and Ti60 alloys
Patent Information
- Application Number
- CN202410357804.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-27
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-03-27
Smart Images

Figure CN118180707B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a brazing method for SiC f Methods for using SiC composite materials with Ti60 alloys. Background Technology
[0002] Ceramic matrix composites are composite materials in which fibers, whiskers, or particulate reinforcing materials are introduced into a ceramic matrix, forming a composite material in which the introduced reinforcing material is the dispersed phase and the ceramic matrix is the continuous phase. SiC f SiC composite materials are novel materials obtained by combining SiC fibers with a SiC matrix. They possess excellent chemical and physical compatibility, with outstanding advantages such as high specific modulus, high specific strength, low coefficient of thermal expansion, high temperature resistance, oxidation resistance, and corrosion resistance. These advantages can improve engine operating temperature and thrust-to-weight ratio. While the addition of silicon carbide fibers can mitigate the inherently poor bending and fracture toughness of ceramics to some extent, the machinability of ceramic matrix composites remains poor, particularly limiting their application in large-scale samples and complex-shaped components. In contrast, metallic materials exhibit diverse and stable physicochemical properties, along with superior machinability and wide versatility. Ti60 alloy, a novel high-temperature titanium alloy, possesses good creep resistance, high high-temperature strength, excellent thermal stability, and high-temperature oxidation resistance, making it a promising candidate material for high thrust-to-weight ratio aero-engine bladed disks. However, at high temperatures, metallic materials suffer structural damage and significant deterioration in performance and strength due to external factors. Therefore, the manufacturing of composite components is necessary to mitigate these shortcomings. Therefore, exploring welding technology between ceramic matrix composites and metals has broad application prospects and profound significance. Summary of the Invention
[0003] This invention aims to address the technical problem of difficult bonding caused by the significant differences in physicochemical properties and coefficients of thermal expansion between ceramic matrix composites and metallic materials. The invention provides a method for brazing SiC using ZrCu solder. f Methods for using SiC composite materials with Ti60 alloys.
[0004] The present invention uses ZrCu solder to braze SiC f The method for combining SiC composite materials with Ti60 alloys is carried out according to the following steps:
[0005] I. Preparation of brazing filler metal: High-purity Zr and Cu blocks were used for arc melting, with an atomic percentage of 1:1 between the two elements. Melting was carried out in a water-cooled copper crucible, and the brazing filler metal was melted 5 to 7 times. After each melting, the metal was cooled to room temperature before the next melting. The melting time for each melting was 55 to 65 seconds. The sample was turned over thoroughly during the melting process. After melting, the metal was cooled to room temperature to obtain an ingot. The brazing filler metal block was then cut into thin slices using a wire cutting machine for later use.
[0006] II. Base Material Preparation: SiC is prepared by wire cutting. f The SiC composite material was cut to the required size, and then the surface to be welded was ground and polished. It was then sanded sequentially with 600#, 1200#, and 1500# wet sandpaper, followed by surface polishing with 0.5μm diamond polishing compound until no obvious scratches remained. The polished SiC... f The SiC composite material was placed in anhydrous ethanol and ultrasonically cleaned for 10-20 minutes, then removed and dried for later use; the Ti60 alloy was treated using the same method.
[0007] 3. Brazing filler metal treatment: Cut the brazing filler metal prepared in step 1 into the required size using an electric discharge wire cutter. Then, polish the surface of the brazing filler metal, and then polish it with 600#, 1200# and 1500# wet sandpaper in sequence. After that, place it in anhydrous ethanol and clean it with ultrasonic vibration for 10 min to 20 min. Take it out and blow it dry for later use.
[0008] 4. Quickly place the ZrCu solder sheet prepared in step 3 onto the SiC substrate prepared in step 2. f The SiC composite material and Ti60 alloy are fixed together using an organic binder to form a SiC composite. f Sandwich structure component consisting of SiC composite material, ZrCu solder, and Ti60 alloy;
[0009] 5. Place the sandwich structure from step 4 into a graphite mold, put it into a vacuum furnace and evacuate it. Under vacuum conditions, first raise the temperature to 300℃~310℃ at 10℃ / min~12℃ / min and hold it for 30min~35min to remove the organic binder. Then raise the temperature to 860℃~870℃ at 10℃ / min~12℃ / min, and then raise the temperature to the brazing temperature of 890℃~950℃ at 5℃ / min~8℃ / min and hold it for 5min~20min. Then lower the temperature to 300℃~310℃ at 5℃ / min~8℃ / min, and finally cool it to room temperature with the furnace to complete the brazing process.
[0010] Advantages of this invention:
[0011] Compared with existing technologies, this invention provides a high-melting-point, low-cost ZrCu solder and achieves SiC synthesis under high vacuum conditions. f The effective bonding between SiC composite materials and Ti60 alloy has the following specific benefits:
[0012] 1. The ZrCu solder provided by this invention is used in SiC f The joining method for SiC composite materials involves using ZrCu solder as an intermediate layer and directly brazing SiC to achieve the desired SiC structure. f The effective connection between SiC composite material and Ti60 alloy, in which ZrCu brazing filler metal has good fluidity, high melting point and excellent wetting properties with the base material, and few defects in the connection layer, is conducive to achieving high-temperature reliability of the joint.
[0013] 2. Compared with traditional TiZrCuNi brazing filler metal, ZrCu brazing filler metal retains the components that are beneficial to the connection process according to the actual base material being brazed, removes the unfavorable compound phases brought about by Ni element, simplifies the complex types of phases generated in the weld, and improves the high temperature resistance of the joint.
[0014] 3. In the connection process of this invention, the brazing filler metal and the base material interact, and SiC... f When the surface of the SiC composite matrix comes into contact with liquid ZrCu solder, the solder penetrates into the SiC matrix. f The pores between fibers or fibers and the matrix in the SiC composite material are filled, and the solder reacts with both the SiC matrix and the SiC fibers to form a new TiC+Ti5Si3 reaction layer. The room temperature shear strength of the joint obtained after holding at 910℃ for 10 min is 40 MPa, the high temperature shear strength at 500℃ is 66 MPa, and the high temperature shear strength at 700℃ is 41 MPa.
[0015] Therefore, this invention uses high-melting-point and low-cost ZrCu solder as an intermediate layer for SiC. f The connection between SiC composite material and Ti60 alloy can achieve good wettability and interfacial bonding of the solder on the base material. This enables low-cost manufacturing of complex components and allows the product components to have different functional characteristics, thus achieving complementary performance between the two. Attached Figure Description
[0016] Figure 1 This is a microstructure diagram of the joint obtained in Example 2;
[0017] Figure 2 For Example 2, an enlarged view of the interface structure of the base materials on both sides of the joint was obtained;
[0018] Figure 3 for Figure 2Elemental composition energy spectrum data of each element at midpoint 1;
[0019] Figure 4 for Figure 2 The elemental composition data of point 2 is shown in the energy spectrum analysis of the content of each element. Detailed Implementation
[0020] Specific Implementation Method 1: This implementation method involves brazing SiC using ZrCu solder. f The method for combining SiC composite materials with Ti60 alloys is specifically carried out according to the following steps:
[0021] I. Preparation of brazing filler metal: High-purity Zr and Cu blocks were used for arc melting, with an atomic percentage of 1:1 between the two elements. Melting was carried out in a water-cooled copper crucible, and the brazing filler metal was melted 5 to 7 times. After each melting, the metal was cooled to room temperature before the next melting. The melting time for each melting was 55 to 65 seconds. The sample was turned over thoroughly during the melting process. After melting, the metal was cooled to room temperature to obtain an ingot. The brazing filler metal block was then cut into thin slices using a wire cutting machine for later use.
[0022] II. Base Material Preparation: SiC is prepared by wire cutting. f The SiC composite material was cut to the required size, and then the surface to be welded was ground and polished. It was then sanded sequentially with 600#, 1200#, and 1500# wet sandpaper, followed by surface polishing with 0.5μm diamond polishing compound until no obvious scratches remained. The polished SiC... f The SiC composite material was placed in anhydrous ethanol and ultrasonically cleaned for 10-20 minutes, then removed and dried for later use; the Ti60 alloy was treated using the same method.
[0023] 3. Brazing filler metal treatment: Cut the brazing filler metal prepared in step 1 into the required size using an electric discharge wire cutter. Then, polish the surface of the brazing filler metal, and then polish it with 600#, 1200# and 1500# wet sandpaper in sequence. After that, place it in anhydrous ethanol and clean it with ultrasonic vibration for 10 min to 20 min. Take it out and blow it dry for later use.
[0024] 4. Quickly place the ZrCu solder sheet prepared in step 3 onto the SiC substrate prepared in step 2. f The SiC composite material and Ti60 alloy are fixed together using an organic binder to form a SiC composite. f Sandwich structure component consisting of SiC composite material, ZrCu solder, and Ti60 alloy;
[0025] 5. Place the sandwich structure from step 4 into a graphite mold, put it into a vacuum furnace and evacuate it. Under vacuum conditions, first raise the temperature to 300℃~310℃ at 10℃ / min~12℃ / min and hold it for 30min~35min to remove the organic binder. Then raise the temperature to 860℃~870℃ at 10℃ / min~12℃ / min, and then raise the temperature to the brazing temperature of 890℃~950℃ at 5℃ / min~8℃ / min and hold it for 5min~20min. Then lower the temperature to 300℃~310℃ at 5℃ / min~8℃ / min, and finally cool it to room temperature with the furnace to complete the brazing process.
[0026] Specific Implementation Method Two: This implementation method differs from Specific Implementation Method One in that the current during arc melting in step one is 200A and the voltage is 30V. Everything else is the same as in Specific Implementation Method One.
[0027] Specific Implementation Method Three: This implementation method differs from Specific Implementation Method One or Two in that the single melting time in step one is 60 seconds. Everything else is the same as in Specific Implementation Method One or Two.
[0028] Specific Implementation Method Four: This implementation method differs from Specific Implementation Methods One to Three in that the ultrasonic oscillation cleaning in step two lasts for 15 minutes. Everything else is the same as in Specific Implementation Methods One to Three.
[0029] Specific Implementation Method Five: This implementation method differs from Specific Implementation Method Four in that the ultrasonic oscillation cleaning in step three lasts for 15 minutes. Everything else is the same as in Specific Implementation Method Four.
[0030] Specific Implementation Method Six: This implementation method differs from Specific Implementation Method Five in that the organic binder mentioned in step four is a hydroxyethyl cellulose solution. Everything else is the same as in Specific Implementation Method Five.
[0031] Specific Implementation Method Seven: This implementation method differs from Specific Implementation Method Six in that the mass fraction of hydroxyethyl cellulose in the hydroxyethyl cellulose solution described in step four is 1%. Everything else is the same as in Specific Implementation Method Six.
[0032] Specific Implementation Method Eight: This implementation method differs from Specific Implementation Method Seven in that the vacuum level in step five is 10. -3 Pa~10 -4 Pa. Everything else is the same as in Specific Implementation Method Seven.
[0033] Specific Implementation Method Nine: This implementation method differs from Specific Implementation Method Eight in that: in step five, the temperature is first raised to 300°C at a rate of 10°C / min under vacuum conditions and held for 30 minutes to remove the organic binder, and then the temperature is raised to 860°C at a rate of 10°C / min. Everything else is the same as in Specific Implementation Method Eight.
[0034] Specific Implementation Method Ten: This implementation method differs from Specific Implementation Method Nine in that: in step five, the temperature is increased to the brazing temperature of 890℃~950℃ at a rate of 5℃ / min and held for 5min~20min; then the temperature is decreased to 300℃ at a rate of 5℃ / min, and finally cooled to room temperature with the furnace to complete the brazing process. Everything else is the same as in Specific Implementation Method Nine.
[0035] The invention was verified using the following experiments:
[0036] Example: A method for brazing SiC using ZrCu solder f The method for combining SiC composite materials with Ti60 alloys is specifically carried out according to the following steps:
[0037] I. Preparation of Brazing filler metal: High-purity Zr and Cu blocks were used for arc melting, with an atomic percentage of 1:1. Melting was carried out in a water-cooled copper crucible, and the filler metal was melted 6 times. After each melting, the metal was cooled to room temperature before the next melting. Each melting time was 60 seconds. The sample was turned frequently during the melting process. After melting, the metal was cooled to room temperature to obtain an ingot. The filler metal block was then cut into 4×4×0.5mm thin slices using a wire cutting machine for later use. The current during arc melting was 200A and the voltage was 30V.
[0038] II. Base Material Preparation: SiC is prepared by wire cutting. f The SiC composite material was cut into 4×4×4mm pieces, and then the surfaces to be welded were ground and polished. This was done sequentially with 600#, 1200#, and 1500# wet sandpaper, followed by polishing with 0.5μm diamond polishing compound until no obvious scratches remained. The polished SiC... f The SiC composite material was placed in anhydrous ethanol and ultrasonically cleaned for 15 minutes. It was then removed, dried, and set aside for use. The Ti60 alloy was treated using the same method.
[0039] 3. Solder treatment: The surface of the solder prepared in step 1 is polished and then polished with 600#, 1200# and 1500# wet sandpaper in sequence. After that, it is placed in anhydrous ethanol and ultrasonically cleaned for 15 minutes. Then it is taken out and dried for later use.
[0040] 4. Quickly place the ZrCu solder sheet prepared in step 3 onto the SiC substrate prepared in step 2. f The SiC composite material and Ti60 alloy are fixed together using an organic binder (a 1% hydroxyethyl cellulose solution) to form a SiC composite. f Sandwich structure component consisting of SiC composite material, ZrCu solder, and Ti60 alloy;
[0041] 5. Place the sandwich structure from step 4 into a graphite mold, put it into a vacuum furnace, and evacuate it to a vacuum level of 10. -3 Pa, under vacuum conditions, first raise the temperature to 300℃ at 10℃ / min and hold for 30min to remove the organic binder, then raise the temperature to 860℃ at 10℃ / min, then raise the temperature to the brazing temperature at 5℃ / min and hold; then lower the temperature to 300℃ at 5℃ / min, and finally cool to room temperature with the furnace to complete the brazing process.
[0042] Six examples were conducted using the process parameters in Table 1 (all process parameters were the same except for those in Table 1), and the room temperature shear strength of the six joints obtained was tested.
[0043] Table 1
[0044]
[0045] As can be seen from Table 1, in Example 2, the room temperature shear strength of the joint obtained by holding at 910℃ for 10 minutes is 40 MPa, the high temperature shear strength at 500℃ is 66 MPa, and the high temperature shear strength at 700℃ is 41 MPa.
[0046] Figure 1 This is a microstructure diagram of the joint obtained in Example 2, where 1 represents SiC. f The figure shows a SiC composite material, 2 is the brazing filler layer, and 3 is Ti60 alloy. As can be seen from the figure, the brazing gap width is about 104μm, with no cracks or defects such as incomplete welding, but there are a small number of closed-cell structures.
[0047] Figure 2 This is an enlarged view of the interface structure of the base materials on both sides of the joint obtained in Example 2, where 1 is SiC. f / SiC composite material, 2 is SiC f The reaction layer formed on the SiC composite side, 3 is the middle part of the weld, 4 is the Ti-based solid solution phase formed on the Ti60 side, and 5 is the Ti60 alloy. f After the SiC composite material and Ti60 alloy base material came into contact with the liquid solder, a small amount of dissolution occurred in both materials. Melting was particularly noticeable at the interface between the two base materials. f A continuous reaction layer is formed on one side of the / SiC composite material, which is beneficial to the performance improvement of the joint. Since Cu is a β-Ti stabilizing element, it can be seen that a β-Ti-rich eutectoid structure is formed on the Ti60 matrix side.
[0048] Figure 3 for Figure 2 The elemental composition at point 1 is analyzed using energy dispersive spectroscopy (EDS) data, which determines the content of each element in SiC based on its composition. fThe reaction layer formed on one side of the / SiC composite material is a TiC+Ti5Si3 phase.
[0049] Figure 4 for Figure 2 The elemental composition energy dispersive spectroscopy data of point 2 shows that, based on the composition, a Ti-based solid solution phase was formed on the Ti60 side due to the diffusion of Ti elements from the base material into the middle of the weld.
Claims
1. A method for brazing SiC using ZrCu solder f The method for using SiC composite materials and Ti60 alloys, characterized in that... Using ZrCu solder to braze SiC f The method for combining SiC composite materials with Ti60 alloys is carried out according to the following steps: I. Preparation of brazing filler metal: High-purity Zr and Cu blocks were used for arc melting, with an atomic percentage of 1:1 between the two elements. Melting was carried out in a water-cooled copper crucible, and the brazing filler metal was melted 5 to 7 times. After each melting, the metal was cooled to room temperature before the next melting. The melting time for each melting was 55 to 65 seconds. The sample was turned over thoroughly during the melting process. After melting, the metal was cooled to room temperature to obtain an ingot. The brazing filler metal block was then cut into thin slices using a wire cutting machine for later use. II. Base Material Preparation: SiC is prepared by wire cutting. f The SiC composite material was cut to the required size, and then the surface to be welded was ground and polished. It was then sanded sequentially with 600#, 1200#, and 1500# wet sandpaper, followed by surface polishing with 0.5μm diamond polishing compound until no obvious scratches remained. The polished SiC... f The SiC composite material parent material was placed in anhydrous ethanol and ultrasonically cleaned for 10-20 minutes. It was then removed, dried, and set aside for use. Ti60 alloy is used in conjunction with the aforementioned SiC. f The same method was used to process the SiC composite material.
3. Brazing filler metal treatment: Cut the brazing filler metal prepared in step 1 into the required size using an electric discharge wire cutter. Then, polish the surface of the brazing filler metal, and then polish it with 600#, 1200# and 1500# wet sandpaper in sequence. After that, place it in anhydrous ethanol and clean it with ultrasonic vibration for 10 min to 20 min. Take it out and blow it dry for later use.
4. Quickly place the ZrCu solder sheet prepared in step 3 onto the SiC substrate prepared in step 2. f The SiC composite material and Ti60 alloy are fixed together using an organic binder to form a SiC composite. f Sandwich structure component consisting of SiC composite material, ZrCu solder, and Ti60 alloy; 5. Place the sandwich structure from step 4 into a graphite mold, put it into a vacuum furnace and evacuate it. Under vacuum conditions, first raise the temperature to 300℃~310℃ at 10℃ / min~12℃ / min and hold it for 30min~35min to remove the organic binder. Then raise the temperature to 860℃~870℃ at 10℃ / min~12℃ / min, and then raise the temperature to the brazing temperature of 890℃~950℃ at 5℃ / min~8℃ / min and hold it for 5min~20min. Then lower the temperature to 300℃~310℃ at 5℃ / min~8℃ / min, and finally cool it to room temperature with the furnace to complete the brazing process.
2. A method for brazing SiC using ZrCu solder according to claim 1 f The method for using SiC composite materials and Ti60 alloys, characterized in that... In step one, the current during arc melting is 200A and the voltage is 30V.
3. A method for brazing SiC using ZrCu solder according to claim 1 f The method for using SiC composite materials and Ti60 alloys, characterized in that... The single melting time in step one is 60 seconds.
4. A method for brazing SiC using ZrCu solder according to claim 1 f The method for using SiC composite materials and Ti60 alloys, characterized in that... In step two, ultrasonic oscillation cleaning is performed for 15 minutes.
5. A method for brazing SiC using ZrCu solder according to claim 1 f The method for using SiC composite materials and Ti60 alloys, characterized in that... In step three, ultrasonic oscillation cleaning is performed for 15 minutes.
6. A method for brazing SiC using ZrCu solder according to claim 1 f The method for using SiC composite materials and Ti60 alloys, characterized in that... The organic binder mentioned in step four is a hydroxyethyl cellulose solution.
7. A method for brazing SiC using ZrCu solder according to claim 6 f The method for using SiC composite materials and Ti60 alloys, characterized in that... The hydroxyethyl cellulose solution described in step four has a hydroxyethyl cellulose mass fraction of 1%.
8. A method for brazing SiC using ZrCu solder according to claim 1 f The method for using SiC composite materials and Ti60 alloys, characterized in that... The vacuum level evacuated in step five is 10. -3 Pa~10 -4 Pa.
9. A method for brazing SiC using ZrCu solder according to claim 1 f The method for using SiC composite materials and Ti60 alloys, characterized in that... Step 5: Under vacuum conditions, first raise the temperature to 300℃ at 10℃ / min and hold for 30 minutes to remove the organic binder, then raise the temperature to 860℃ at 10℃ / min.
10. A method for brazing SiC using ZrCu solder according to claim 1 f The method for using SiC composite materials and Ti60 alloys, characterized in that... In step five, the temperature is increased to the brazing temperature of 890℃~950℃ at a rate of 5℃ / min and held for 5min~20min; then the temperature is decreased to 300℃ at a rate of 5℃ / min, and finally cooled to room temperature with the furnace to complete the brazing process.
Citation Information
Patent Citations
Connecting method for Cf / SiC composite material and titanium alloy
CN101462890A
Brazing filler metal for SiCf / SiC composite material connection and brazing connection method