A metal-resin combination based on bionic micro-nano structure enhancement and a preparation method thereof
By constructing biomimetic micro/nano structures on metal surfaces and using silane coupling agents to form covalent bonds, the problem of low bonding strength between metals and resins was solved, achieving higher bonding strength and a simpler process.
Patent Information
- Application Number
- CN202410289747.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-14
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-03-14
AI Technical Summary
Existing technologies are insufficient to effectively improve the bonding strength between metals and resins. Traditional methods suffer from problems such as low bonding strength, complex processes, and poor acid and alkali resistance.
A biomimetic micro/nano structure enhancement method is adopted. By constructing biomimetic micro/nano structures on the metal surface and forming covalent bonds using silane coupling agents, combined with laser etching and chemical etching techniques, metal-resin composites are prepared.
It significantly improves the bonding strength between resin and metal, achieving stronger anchor connections and uniform coating, and simplifies the process.
Smart Images

Figure CN118181732B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a metal composite material and its preparation method, and particularly to a metal resin composite material reinforced by a biomimetic micro / nano structure and its preparation method. Background Technology
[0002] With societal progress, the limitations of single-material applications are becoming increasingly apparent. Metals, due to their high strength, hardness, and excellent electrical conductivity, are widely used, but their high density and poor corrosion resistance limit their further applications. In contrast, resins possess advantages such as high specific strength, good moldability, and electrical insulation, but they suffer from poor heat resistance, susceptibility to aging, low stiffness, and a large coefficient of thermal expansion. Therefore, composite materials that combine the advantages of different materials are increasingly becoming a focus of attention. The technology of integrating metals and resins has significant application potential in a wide range of industrial sectors, including aerospace, automotive, and marine industries. However, in practical applications, the problem of bonding metals and resins often needs to be solved.
[0003] Traditional solutions involve using adhesives or creating numerous rivets, buckles, and holes. However, these methods all have some problems, such as poor acid and alkali resistance of adhesives, making it impossible to perform subsequent surface treatments on the composite; using riveting methods not only increases the process flow but also results in larger product sizes and lower bonding strength of the resulting metal-resin composite.
[0004] In addition, anodizing is used to etch nanoscale alumina pores on the surface of aluminum alloys, and then bond them with resin to form an aluminum-plastic composite. However, the pores on the surface of the aluminum alloy obtained by this method are single columnar, and the molten resin cannot easily penetrate completely into the nanopores. The force between the resin and the oxide layer is weak, and the plastic and metal can easily fall off under the action of force, which reduces the bonding strength between the aluminum alloy and the resin, i.e., the tensile properties are poor.
[0005] Therefore, improving the bonding strength between metal and resin has become a key aspect in the development of metal / resin composite materials. There is an urgent need to develop a metal-resin composite material and its preparation method that takes into account bonding strength, environment, and time. Summary of the Invention
[0006] Objectives of the invention: The first objective of the present invention is to provide a metal-resin composite based on biomimetic micro-nano structure reinforcement to improve the bonding strength between resin and metal; the second objective of the present invention is to provide a method for preparing the metal-resin composite based on biomimetic micro-nano structure reinforcement.
[0007] Technical solution: The metal-resin composite based on biomimetic micro-nano structure enhancement described in this invention includes a metal layer and a resin layer, wherein the surface where the metal and resin are connected has a biomimetic micro-nano structure.
[0008] By constructing biomimetic micro / nano structures, the wettability between the resin and the metal surface is improved, which helps to achieve a uniform coating of resin on the metal surface. Preferably, the biomimetic micro / nano structure is a shark-scale-like structure, i.e., a secondary rib structure, such as... Figure 1 As shown. The primary ribs are located at the bottom layer and are distributed in an alternating pattern of continuous and discontinuous ribs. The secondary ribs are ribs with smaller widths built on top of the primary ribs.
[0009] Preferably, the surface of the biomimetic micro / nanostructure has a film formed by a silane coupling agent with amino groups. Introducing the silane coupling agent onto the metal surface causes silanization of the metal surface, generating a large number of amino groups to promote covalent bonding between the metal surface and the resin. Preferably, the amino-containing silane coupling agent is KH-540.
[0010] Preferably, the surface of the biomimetic micro / nano structure has micro / nano-level pores, which can easily form a nano-anchor effect with the resin.
[0011] In this invention, the resin may be a conventional epoxy resin in the art, such as E51 epoxy resin.
[0012] In this invention, the metal can be a conventional metal or alloy in the art, such as 5083 aluminum alloy.
[0013] The method for preparing the metal-resin composite of the present invention is characterized by comprising the following steps:
[0014] (1) Remove impurities from the metal surface;
[0015] (2) Laser scanning etching is used to process the metal surface to form a biomimetic micro-nano structure;
[0016] (3) Use a polyacid solution to treat the photo-etched metal surface to corrode and generate holes;
[0017] (4) The acid-treated metal surface is subjected to silanization treatment. An amino-containing silane coupling agent solution is sprayed onto the metal surface and then condensed into a film.
[0018] (5) A diluted solution of resin for coating the metal surface after silanization treatment;
[0019] (6) Cast resin in a mold, then bring the side of the metal with micro-nano structure into contact with the resin, and finally cure to form an integrated metal-resin composite.
[0020] When the surface of the biomimetic micro / nano structure does not have micro / nano-level pores, step (3) is not performed; when the surface of the biomimetic micro / nano structure does not have a film formed by an amino-containing silane coupling agent, step (4) is not performed.
[0021] Preferably, in step (1), the method for removing impurities from the metal surface is: alkaline etching treatment, in which the metal substrate is immersed in an alkaline solution to completely cover the metal substrate. The alkali can be one or more of sodium bicarbonate, potassium bicarbonate, sodium carbonate, potassium carbonate, sodium hydroxide, and potassium ammonia. More preferably, the alkali is sodium hydroxide, the solution concentration is 60 g / L to 70 g / L, the solution temperature is 60 to 70 °C, and the treatment time is 3 to 5 min.
[0022] Preferably, in step (2), the laser scanning etching conditions are: laser power 20W, spot diameter 0.02mm, scanning spacing 0.04~0.06mm, and scanning speed 100~1000mm / s.
[0023] The polyacid solution treatment process can effectively remove micro- and nano-sized particulate impurities formed by molten sputtering after laser etching. Furthermore, this process can create micro- and nano-sized pores on the metal surface, and these nanostructures can easily form a nano-anchor effect with the resin. Preferably, the polyacid is a mixture of sulfuric acid and nitric acid.
[0024] More preferably, the mass fraction of sulfuric acid in the polyacid solution is 20-30%, the mass fraction of nitric acid is 30-35%, and the remainder is water; the solution temperature is 40-60℃, and the treatment time is 2-5 min.
[0025] After the silanization process, a silane coupling agent solution is sprayed onto the metal surface. After solidification, a silane coupling film with amino groups (-NH2) is cured on the metal surface and porous structure. The silane coupling agent is introduced onto the metal surface to promote the formation of covalent bonds between the metal surface and the resin.
[0026] Preferably, in step (4), the solvent for the amino-containing silane coupling agent solution is a mixture of ethanol and water. Preferably, the silane coupling agent solution is a hydrolysate obtained by mixing KH-540, deionized water, and ethanol in a weight ratio of 1–5:1–5:90–98 and stirring at room temperature for 40 minutes.
[0027] Preferably, in step (4), the condensation film formation method is: heating and drying at 100-120°C for 1-3 hours.
[0028] In step (5), the resin diluent coating is more conducive to the resin penetration into the micro-nano structure of the metal surface, so as to achieve a stronger anchor bolt connection.
[0029] Preferably, in step (5), the resin diluent is a mixture of resin and acetone, and the resin accounts for 5% to 20% of the total mass of the resin solution, with the remainder being acetone.
[0030] Preferably, the method for preparing the resin diluent includes: first pouring acetone into a container, then adding resin, and stirring until the solution is clear and free of precipitate for 60-90 seconds to obtain the resin diluent. More preferably, the resin diluent is applied to the bonding interface of the substrate within 30 minutes of preparation.
[0031] Preferably, the resins used in steps (5) and (6) are the same type of resin.
[0032] Preferably, in step (5), the coating includes dipping, brushing or spraying, which can be selected according to the shape, size and processing technology of the sample.
[0033] In step (6), the resin is a pure resin or a resin-filler reinforced resin system.
[0034] Preferably, in the reinforced resin system, the resin accounts for 90-100% of the resin mass percentage, and the filler accounts for 0-10% of the resin mass percentage.
[0035] Preferably, the reinforcing material can be at least one of glass fiber, carbon fiber, and aramid fiber.
[0036] The amount of resin used in this invention is not specifically limited. It can be determined according to the size of the mold and the size of the metal matrix, as long as the metal matrix and the resin composition can be integrated into a metal-resin composite.
[0037] In step 6, the curing process includes pre-curing and secondary curing. The secondary curing involves reducing the resin curing time through high-temperature baking; the secondary curing temperature and time can be determined based on the selected resin matrix. Alternatively, room-temperature curing can be achieved by extending the secondary curing time. Preferably, the applicable curing temperature for epoxy resin E-51 is 60–100°C, and the curing time is 30–150 minutes.
[0038] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) The metal-resin composite material successfully improves the wettability of the resin and the metal surface by constructing a biomimetic micro-nano structure on the metal and resin surfaces, which helps to achieve a uniform coating of resin on the metal surface and introduce silane coupling agent on the metal surface to promote the formation of covalent bond connection between the metal surface and the resin; (2) This method combines laser melting and chemical corrosion technology, which can obtain high-quality and controllable alloy surface micro-nano structures compared with traditional methods; (3) The resin solution coating strategy is more conducive to the resin penetrating into the metal surface micro-nano structure to achieve a stronger anchor connection; (4) This method is simple to operate and has high process feasibility. Attached Figure Description
[0039] Figure 1This is a schematic diagram of a shark-like dermal shield structure.
[0040] Figure 2 For laser etching processing patterns and dimensions;
[0041] Figure 3 This is a morphology image of the metal surface obtained by laser etching in Example 1;
[0042] Figure 4 The image shows the surface morphology of the metal obtained by silanization in Example 1.
[0043] Figure 5 XPS spectra of the metal surface obtained by silanization in Example 1;
[0044] Figure 6 XPS spectra of the metal surface obtained by silanization in Comparative Example 2;
[0045] Figure 7 XPS images of the metal surface obtained by pickling in Comparative Example 3. Detailed Implementation
[0046] The technical solution of the present invention will be further described below with reference to the embodiments.
[0047] The biomimetic micro / nano structure-enhanced metal-resin composite and its preparation method of the present invention include the following steps:
[0048] (1) Select a standard size 5083 aluminum alloy plate, immerse the aluminum alloy plate in sodium hydroxide solution, so that the sodium hydroxide solution completely covers the metal substrate of the step. The concentration of sodium hydroxide solution is 70g / L, the solution temperature is 60℃, and the treatment time is 4min.
[0049] (2) The aluminum alloy surface obtained in step (1) was etched by laser scanning. The laser processing conditions were: laser power 20W, spot diameter 0.02mm, scanning spacing 0.04, and scanning speed 1000mm / s. The processing dimensions and patterns are as follows: Figure 2 As shown, the laser processing fill interval is 0.01 mm, the length of a single secondary rib processing unit is 290 μm and the width is 200 μm; the width of the primary rib is 50 μm, and the width of the secondary rib is 15 μm; the length of the continuous rib is 290 μm, and the length of the discontinuous rib is 174 μm; since laser processing is a subtractive process, in the laser etching preparation process, first according to... Figure 2 (a) shows the machining of the secondary ribs, and then according to... Figure 2 (b) The diagram shows the machining of the first-level rib.
[0050] (3) Immerse the aluminum alloy surface obtained in step (2) in a polyacid solution at a temperature of 40°C for 5 minutes. The polyacid solution contains 28% sulfuric acid, 34% nitric acid, and the remainder is water.
[0051] (4) Mix silane coupling agent (KH-540), deionized water and ethanol in a weight ratio of 5:5:90, stir at room temperature for 40 min to obtain a hydrolysis solution, spray the hydrolysis solution evenly onto the aluminum alloy surface obtained in step (3), and bake at 120°C for 2 hours to form a silane coupling agent film.
[0052] (5) Mix E-51 epoxy resin and acetone at a weight ratio of 10:90 to form a resin solution, and apply the solution evenly to the aluminum alloy surface obtained in step (4).
[0053] (6) Mix carbon fiber, E-51 epoxy resin and curing agent (triethylenetetramine) in a weight ratio of 3:100:15 and pour them into a mold. Then place the metal surface treated in step (5) face down in the mold to form a metal-resin composite.
[0054] (7) Place the pre-cured aluminum alloy resin composite into an oven for secondary curing. The curing temperature is 70℃ and the curing time is 120min.
[0055] Example 2
[0056] The metal / resin composite was prepared using the same method as in Example 1, except that no silane coupling agent was applied in step (4).
[0057] Example 3
[0058] The metal / resin composite was prepared using the same preparation method as in Example 2, except that acid washing was not performed in step (3).
[0059] Comparative Example 1
[0060] The metal / resin composite was prepared using the same method as in Example 1, except that laser etching was not performed in step (2), and the metal surface lacked biomimetic micro / nano structures. XPS spectral analysis was performed on it as follows: Figure 5 As shown.
[0061] Comparative Example 2
[0062] The metal / resin composite was prepared using the same method as Comparative Example 1, except that polybasic acid cleaning was not performed in step (3). XPS spectra analysis were performed on it as follows: Figure 6 As shown.
[0063] Comparative Example 3
[0064] The metal / resin composite was prepared using the same method as Comparative Example 1, except that no silane coupling agent was applied in step (4). XPS spectra were analyzed as follows: Figure 7 As shown.
[0065] Comparative Example 4
[0066] The metal / resin composite was prepared using the same preparation method as in Example 1, except that steps (1) to (4) were omitted, i.e., the metal surface was not treated.
[0067] Structural characterization
[0068] Example 1 Step (2) Morphology after laser etching is as follows Figure 3 As shown.
[0069] Depend on Figure 3 It can be seen that the shark-scale-like structure presents a two-stage rib structure distribution. According to the groove distribution in the figure, it can be observed that the primary ribs are distributed in an alternating pattern of continuous and discontinuous ribs. The secondary ribs are processed on the primary ribs, and the secondary rib structure with a smaller width is obtained by laser etching grooves.
[0070] Example 1: After step (4) silane coupling treatment, the morphology of the silane coupling agent film formed on the metal surface is as follows: Figure 4 As shown.
[0071] Depend on Figure 4 It can be seen that, in the mesoscopic state, the metal surface is covered with an irregularly distributed band-like material, which is formed by the hydrolysis and condensation of silane coupling agent. Part of the morphology of the metal surface is covered and filled by the silane hydrolysis and condensation product, indicating that the silane coupling agent has been successfully loaded onto the metal surface.
[0072] XPS spectra analysis was performed on Example 1, Comparative Example 2, and Comparative Example 3 as follows: Figures 5-7 As shown.
[0073] Figure 5 , Figure 6 , Figure 7 The comparison shows that different treatments alter the distribution of elements on the metal surface. For example... Figure 5 As shown, the oxygen content on the surface of aluminum alloys that have not undergone multi-acid treatment is relatively low. Figure 7 As shown, the relative oxygen content on the surface of the aluminum alloy increases significantly after treatment with multi-component acids. Figure 5 As shown, the relative oxygen content on the aluminum alloy surface decreased again after treatment with a polybasic acid followed by the application of a silane coupling agent. It can be inferred that the polybasic acid, while removing oxides from the aluminum alloy surface, formed a higher-quality oxide layer, increasing the oxygen content. After applying the silane coupling agent, the silane coupling agent reacted with the hydroxyl and carboxyl groups on the aluminum alloy surface, further consuming the oxygen on the surface. XPS spectral analysis confirmed that the silane coupling agent was successfully applied to the aluminum alloy surface.
[0074] Test case
[0075] After the metal / resin composites obtained in Example 1 and Comparative Examples 1-6 were left to stand for 6 hours, they were fixed on a universal testing machine for tensile testing. The average shear force in the test results can be regarded as the magnitude of the bonding force between the metal matrix and the resin. The test results are shown in Table 1.
[0076] Table 1 Shear strength of Example 1 and Comparative Examples 1-6
[0077] Metal / resin composite Mean shear force (MPa) Example 1 12.52 Example 2 8.175 Example 3 7.755 Comparative Example 1 1.38 Comparative Example 2 1.3 Comparative Example 3 1.55 Comparative Example 4 0.496
[0078] As can be seen from the data in Table 1, the average shear force of the metal / resin composites prepared in Examples 1 to 3 is significantly higher than that of the metal / resin composites prepared in Comparative Example 1, indicating that surface treatment of metals can effectively improve shear force.
[0079] As can be seen from the comparison between Example 1 and Examples 2 and 3, further acid washing and silanization treatment of the bonding surface can better bring out the excellent performance of the biomimetic micro-nano structure and further improve the shear force.
[0080] The average shear force of the metal / resin composites in Examples 1-3 was significantly enhanced compared to the average shear force of the metal / resin composites prepared in Comparative Examples 1-3, indicating that the biomimetic micro / nano structures prepared by the present invention have good effects.
Claims
1. A metal-resin composite reinforced with biomimetic micro / nano structures, characterized in that, It includes a metal layer and a resin layer, and the surface where the metal and resin are connected has a biomimetic micro / nano structure; the biomimetic micro / nano structure is a shark-like shield scale structure. The biomimetic micro / nano structure is a two-stage rib structure, in which the primary rib is located at the bottom layer and is distributed in an alternating pattern of continuous and discontinuous ribs. The secondary rib is a rib with a smaller width that is built on top of the primary rib.
2. The metal-resin composite according to claim 1, characterized in that, The surface of the biomimetic micro / nano structure has a film formed by an amino-containing silane coupling agent.
3. The metal-resin composite according to claim 1, characterized in that, The surface of the biomimetic micro / nano structure has micro / nano-level pores.
4. The method for preparing a resin conjugate according to claim 2, characterized in that, The amino-containing silane coupling agent is KH-540.
5. A method for preparing the metal-resin composite according to any one of claims 1 to 4, characterized in that, Includes the following steps: (1) Remove impurities from the metal surface; (2) Laser scanning etching is used to process the metal surface to form a biomimetic micro / nano structure; (3) Use a polyacid solution to treat the laser-etched metal surface to generate micro-nano-scale pores; (4) The acid-treated metal surface is subjected to silanization treatment. An amino-containing silane coupling agent solution is sprayed onto the metal surface and then condensed into a film. (5) Coating the silanized metal surface with a resin diluent; (6) Cast resin in a mold, then bring the side of the metal with micro-nano structure into contact with the resin, and finally cure to form an integrated metal-resin composite. When the surface of the biomimetic micro / nano structure does not have micro / nano-level pores, step (3) is not performed; when the surface of the biomimetic micro / nano structure does not have a film formed by an amino-containing silane coupling agent, step (4) is not performed.
6. The method for preparing a resin conjugate according to claim 5, characterized in that, In step (2), the laser scanning etching conditions are: laser power 20 W, spot diameter 0.02 mm, scanning spacing 0.04~0.06 mm, and scanning speed 100~1000 mm / s.
7. The method for preparing a resin conjugate according to claim 5, characterized in that, The polyacid is a mixture of sulfuric acid and nitric acid.
8. The method for preparing a resin conjugate according to claim 7, characterized in that, The polyacid solution contains 20-30% sulfuric acid and 30-35% nitric acid, with the remainder being water; the solution temperature is 40-60℃, and the treatment time is 2-5 min.
9. The method for preparing a resin conjugate according to claim 5, characterized in that, In step (4), the solvent of the amino-containing silane coupling agent solution is a mixture of ethanol and water.
Citation Information
Patent Citations
Metal-resin compound and preparation method thereof
CN105729717A
Metal matrix surface bionic micro-structure reinforced fiber metal laminate
CN112810250A
Method for fabricating metal-plastic combination using chemical etching
KR1020160117666A