A hydrogenation catalyst and a method for preparing the same

By adjusting the pH of the metal salt solution below the zero charge point of the support, the dispersion of the metal on the support is improved. Sulfidation and carbonization passivation treatments are then performed, which solves the problems of spontaneous combustion risk and carbonization control of sulfided hydrogenation catalysts, improves the safety and activity of the catalyst, and extends its service life.

CN118204131BActive Publication Date: 2026-11-20PETROCHINA CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211622231.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-16
Publication Date
2026-11-20
Estimated Expiration
2042-12-16

AI Technical Summary

Technical Problem

In the existing technology, sulfurized hydrogenation catalysts are at risk of spontaneous combustion when exposed to O₂ in the air, and the carbon deposits on the catalyst surface are difficult to control after carbon passivation treatment, resulting in the permanent loss of some hydrogenation active sites.

Method used

By adjusting the pH of the metal salt solution below the zero point of charge of the support, a strong charge adsorption effect is formed between the metal salt and the support, thereby improving the dispersion of the metal on the support. Subsequently, sulfidation and carbonization passivation treatments are carried out to control the type and degree of carbonization and ensure the safety and activity of the catalyst.

Benefits of technology

This approach enhances catalyst safety, avoids risks associated with container transportation, shortens refinery start-up time, and extends catalyst lifespan, resulting in significant economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004002877890000171
    Figure BDA0004002877890000171
  • Figure BDA0004002877890000172
    Figure BDA0004002877890000172
  • Figure BDA0004002877890000173
    Figure BDA0004002877890000173
Patent Text Reader

Abstract

The application provides a hydrogenation catalyst and a preparation method thereof, and the preparation method comprises the following steps: impregnating a carrier with a metal salt solution, drying, calcining, and obtaining a shaped catalyst; wherein the pH value of the metal salt solution is lower than the zero point of zeta potential of the carrier; performing sulfidation treatment on the shaped catalyst to obtain a sulfidation state catalyst; and performing passivation treatment on the sulfidation state catalyst by using a carbon-containing passivation agent to obtain the hydrogenation catalyst, which is beneficial to controlling the type and degree of carbon deposition, improving the safety of catalyst transportation and loading, and ensuring that the catalyst activity is not reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of catalyst technology, specifically relating to a hydrogenation catalyst and its preparation method. Background Technology

[0002] Because sulfide-form hydrogenation catalysts have high initial activity, they generate SO2 and heat when exposed to air and encounter O2, posing a risk of spontaneous combustion. Therefore, it is necessary to passivate sulfide-form hydrogenation catalysts to suppress their excessively high initial activity.

[0003] Currently, carbon deposition passivation is commonly used to treat sulfide-state hydrogenation catalysts. For example, patent document CN113908888A discloses a passivation method that uses gaseous olefins and CO to carbonize and passivate the catalyst. However, the carbon deposition on the surface of the catalyst after passivation is difficult to control, which can easily lead to the permanent loss of some hydrogenation active sites.

[0004] Therefore, how to provide an off-site sulfided hydrogenation catalyst that has controllable carbon deposition, safe transportation, and no reduction in catalyst activity is a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0005] The method for preparing the hydrogenation catalyst provided by this invention improves the dispersion of the metal on the support by adjusting the pH value of the metal salt solution to be lower than the zero point of charge of the support, and then performing sulfidation treatment and carbonization passivation treatment in sequence. This helps to control the type and degree of carbonization, improve the safety of the catalyst, and ensure that the catalyst activity is not reduced, especially the safety of transportation and loading.

[0006] The hydrogenation catalyst provided by this invention, prepared by the above-described method, exhibits excellent performance in terms of safety and catalytic activity. It avoids container transportation, which helps to shorten refinery start-up time, extend catalyst life, and results in significant economic benefits.

[0007] In one aspect, the present invention provides a method for preparing a hydrogenation catalyst, comprising the following steps:

[0008] A shaped catalyst is obtained by impregnating a support with a metal salt solution, followed by drying and calcination; wherein the pH value of the metal salt solution is lower than the zero point of charge of the support.

[0009] The shaped catalyst is subjected to sulfidation treatment to obtain a sulfidated catalyst;

[0010] A hydrogenation catalyst was obtained by passivating a sulfidated catalyst with a carbon-containing passivating agent.

[0011] According to one embodiment of the present invention, the zero point of the carrier is obtained by a method comprising the following steps: mixing the carrier with deionized water to form a suspension of 0.4 g / L, and adjusting the pH of the suspension to bring the zeta potential of the suspension to zero.

[0012] When the zeta potential of the suspension reaches zero, the pH value of the suspension is the zero electrical point of the carrier.

[0013] According to one embodiment of the present invention, the molding catalyst is subjected to the sulfidation treatment under the combined action of a sulfiding agent and hydrogen; wherein the sulfiding agent includes at least one of hydrogen sulfide, mercaptan, carbon disulfide, dimethyl sulfide, dimethyl disulfide, and phenyl thio compounds.

[0014] According to one embodiment of the present invention, the conditions for vulcanization treatment are: temperature of 200-400°C, pressure of 0.1-3.0 MPa, and time of 2-20 h.

[0015] According to one embodiment of the present invention, the sulfidated catalyst is contacted with a mixture of an inert gas and a carbon-containing passivating agent to perform the passivation treatment;

[0016] In the mixed gas, the volume concentration of the carbon passivating agent is 1%-10%.

[0017] According to one embodiment of the present invention, the carbon-containing passivating agent is selected from at least two of carbon dioxide, C1-C4 alkanes, C2-C4 alkenes, and C2-C4 alkynes.

[0018] According to one embodiment of the present invention, the passivation treatment conditions are: temperature 350℃~450℃, pressure 0.5MPa~3.5MPa, and volume hourly space velocity 500h⁻¹. -1 ~10000h -1 The time is 2 hours to 10 hours.

[0019] According to one embodiment of the present invention, the metal salt solution includes at least one metal element from Group VIB and Group VIII of the periodic table.

[0020] According to one embodiment of the present invention, the drying conditions are: temperature 80-140°C, time 2-6 hours; and / or,

[0021] The calcination conditions are: temperature 400-700℃, time 4-8h.

[0022] In a second aspect, the present invention provides a hydrogenation catalyst prepared by the above-described preparation method.

[0023] The implementation of this invention has at least the following beneficial effects:

[0024] The method for preparing the hydrogenation catalyst provided by this invention involves adjusting the pH value of the metal salt solution below the zero charge point of the support, allowing the negatively charged metal salt to adsorb onto the positively charged support surface. This results in both solid-liquid adsorption and strong charge adsorption between the metal salt and the support, leading to a stronger support-metal interaction in the prepared catalyst. This process is beneficial for improving the dispersion of the active metal component on the support. Sulfidation treatment is then performed to activate the metal sites, further enhancing catalyst activity. Finally, a carbonization passivation treatment is conducted. Due to the high dispersion of the active metal component in the prepared catalyst, the carbonization passivation process helps alleviate excessive carbon buildup on the catalyst surface, while also obtaining easily removable α-carbon, improving catalyst safety while ensuring that catalyst activity does not decrease. Attached Figure Description

[0025] Figure 1 This is a diagram showing the charge adsorption interaction between the metal salt solution and the carrier;

[0026] Figure 2 These are TEM images of different types of carbon; where a is a TEM image of graphitic carbon; b is a TEM image of filamentous carbon at one magnification; c is a TEM image of spherical encapsulated carbon; and d is a TEM image of filamentous carbon at another magnification.

[0027] Figure 3 These are the hydrogen consumption peak temperatures of different types of carbon. Based on the level of the hydrogen consumption peak temperature, carbon deposits are classified into C1 and C2. α C β and C γ Three types, C α The peak temperature for hydrogen consumption is 230℃-380℃; C β The peak temperature for hydrogen consumption is 380℃-500℃; C γ The peak temperature for hydrogen consumption is 500℃-730℃. Detailed Implementation

[0028] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions in the embodiments of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only some embodiments of this invention, not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

[0029] In a first aspect, the present invention provides a method for preparing a hydrogenation catalyst, comprising the following steps: impregnating a support with a metal salt solution, followed by drying and calcination to obtain a shaped catalyst; wherein the pH value of the metal salt solution is lower than the zero point of charge of the support; subjecting the shaped catalyst to sulfidation treatment to obtain a sulfidated catalyst; and passivating the sulfidated catalyst with a carbon-containing passivating agent to obtain a hydrogenation catalyst.

[0030] This invention does not limit the specific type of metal salt solution, as long as it contains an active metal with catalytic activity. This invention also does not limit the specific type of support, which can be a conventional catalyst support in the art. For example, the support includes, but is not limited to, at least one of alumina, zirconium oxide, silicon oxide, activated carbon, diatomaceous earth, and zeolite.

[0031] In this invention, the zero point of charge of the carrier refers to the pH value corresponding to the zero charge of the carrier suspension, wherein the carrier suspension is a mixture of carrier and water.

[0032] The active metal component in the metal salt solution is loaded onto the support by impregnating it with a metal salt solution. After drying and calcination, a shaped catalyst is obtained. At this time, the active metal component in the shaped catalyst exists in the form of oxidation.

[0033] After the shaped catalyst undergoes sulfidation treatment, the oxidized active metal components are transformed into sulfidated active metal components, enabling the catalyst's catalytic activity and stability to meet production requirements.

[0034] This invention does not limit the sulfidation treatment and can select the appropriate method according to actual needs. For example, the sulfiding agent can be introduced into the pores of the molding catalyst by sublimation, melting, or impregnation, so that the molding catalyst and the sulfiding agent combine. Then, hydrogen gas or hydrogen gas and oil are introduced simultaneously, and the sulfidation treatment of the molding catalyst is completed as the temperature rises. Alternatively, hydrogen sulfide or easily decomposable organic sulfides can be used as sulfiding agents. Within a certain temperature, pressure, and space velocity range, hydrogen sulfide or hydrogen sulfide generated by the decomposition of organic sulfides reacts with the molding catalyst to complete the sulfidation treatment of the catalyst.

[0035] This invention does not limit the passivation treatment; it can be conventional carbon deposition passivation in the art. After passivation, carbon deposits form on the surface of the sulfide-state active metal component, preventing the sulfide-state active metal component from contacting air and reducing the hazard of the hydrogenation catalyst.

[0036] According to the technical solution of the present invention, by adjusting the pH value of the metal salt solution below the zero electrical point of the support, the dispersion of the metal on the support is improved. Then, sulfidation and carbonization passivation treatments are performed sequentially. This facilitates control over the type and degree of carbon deposition, improving catalyst safety while ensuring that catalyst activity does not decrease. Based on this phenomenon, the inventors believe that the dispersion of the active metal component on the support significantly affects the catalytic performance of the hydrogenation catalyst, and also influences the type and degree of carbon deposition formed during the subsequent passivation treatment. This invention adjusts the pH of the metal salt solution below the zero point of charge of the support, causing the metal salt to exist in the form of negative ions. At this time, the support surface presents a positive charge, making full use of the strong electron adsorption between the metal salt and the support in the metal salt solution. This allows the metal salt to be highly spread on the support surface or attached to the support pores. After drying and calcination, the active metal components are highly dispersed and loaded on the support, which is beneficial to improving the catalytic activity of the catalyst. Then, a sulfidation treatment is performed to activate the metal sites and further enhance the catalytic activity of the catalyst. Finally, a carbonization passivation treatment is performed. Due to the high dispersion of the active metal components on the support, the carbonization passivation process helps to alleviate the phenomenon of excessive carbonization on the catalyst surface, and at the same time, easily removable α-carbon (filamentous carbon) is obtained, which improves the safety of the catalyst while ensuring that the catalyst activity does not decrease.

[0037] Furthermore, the zero-point electrical potential (ZET) of the carrier is obtained by a method comprising the following steps: mixing the carrier with deionized water to form a 0.4 g / L suspension, adjusting the pH of the suspension to bring its Zeta potential to zero; the pH value at which the Zeta potential of the suspension reaches zero is the zero-point electrical potential of the carrier. For example, γ-Al₂O₃ powder is dissolved in deionized water to prepare a 0.4 g / L γ-Al₂O₃ suspension, the pH of the suspension is adjusted, and its Zeta potential is measured. The pH value corresponding to the zero Zeta potential of the suspension is the zero-point electrical potential of γ-Al₂O₃.

[0038] By adjusting the pH of the metal salt solution below the zero point of charge of the support, the negatively charged metal salt can be adsorbed onto the positively charged support surface. This results in both liquid-solid adsorption and strong charge adsorption between the metal salt and the support, thus giving the prepared catalyst a strong support-metal interaction. Specifically, taking molybdenum salt as an example, for instance... Figure 1 As shown, when the pH of the metal salt solution is lower than the zero charge point of the carrier, the molybdenum salt in the metal salt solution reacts as Mo7O. 24 6- In its current form, the carrier surface is positively charged, and the molybdenum salt and the carrier are strongly adsorbed by the positive and negative charges, which is beneficial for achieving a high degree of dispersion of the active metal component. When the pH value of the metal salt solution is higher than the zero point of charge of the carrier, the carrier surface is negatively charged, and the molybdenum salt in the metal salt solution exists as MoO4.2- The negative ions repel each other, resulting in weak interaction between the metal ions and the carrier, which is not conducive to the dispersion of the metal on the carrier surface.

[0039] In one embodiment of the present invention, the molding catalyst is subjected to sulfidation treatment under the combined action of a sulfiding agent and hydrogen, so that the sulfiding agent entering the pores of the molding catalyst comes into contact with hydrogen. At this time, the sulfiding agent reacts with hydrogen to generate hydrogen sulfide, and the active metal component in the molding catalyst in the oxidized form reacts with hydrogen sulfide to form a sulfidated active metal component.

[0040] The sulfiding agent includes hydrogen sulfide and / or easily decomposable organic sulfides. Further, the organic sulfides include at least one of thiols, carbon disulfide, dimethyl sulfide, dimethyl disulfide, and phenylthio compounds.

[0041] This invention does not limit the amount of sulfiding agent added, as long as sulfidation can be achieved. In one embodiment of this invention, the amount of sulfiding agent added satisfies the requirement that the volume fraction of hydrogen sulfide in the reactor is 1-3%.

[0042] This invention does not impose excessive limitations on the relevant parameters in the vulcanization process, as long as the vulcanization process can be completed. In one embodiment of this invention, the vulcanization conditions are: temperature 200-400℃, pressure 0.1-3.0MPa, and time 2-20h.

[0043] The aforementioned sulfidation treatment is a gas-solid phase reaction process that can be carried out in reactors such as fluidized beds, fixed beds, spouted beds, and moving beds. For example, a granular, molded catalyst is packed into the sulfidation reactor to form a fixed bed of a certain height. The reactor is then purged with inert gas to maintain a temperature of 40-100°C for 1-5 hours. Next, a sulfiding agent and hydrogen gas at a specific temperature are introduced into the reactor, and sulfidation is achieved as the sulfiding agent and hydrogen gas flow through the fixed bed. The temperature of the sulfiding agent can be 160-180°C, and the reactor heating rate is 20-30°C / h.

[0044] This invention employs the aforementioned in-situ reaction to sulfide the formed catalyst, which eliminates the diffusion resistance of the formed catalyst, resulting in more thorough sulfide treatment and improved utilization of the active metal components. Furthermore, it avoids pollutant emissions, shortens start-up time, alleviates safety and environmental pressures, and improves economic efficiency.

[0045] In this invention, the active metal component in the sulfidated catalyst exists in the sulfidated state and has high activity. After sulfidation treatment, there is no need to cool down. The sulfidated catalyst can be directly passivated using a carbon-containing passivating agent, which can make the metal active sites on the surface of the sulfidated catalyst covered by carbon deposits, suppressing its high activity in the early stage and ensuring the safety of the catalyst.

[0046] The carbon-containing passivating agent is preferably a gaseous passivating agent, which facilitates sufficient contact between the sulfide-state catalyst and the carbon-containing passivating agent. For example, the carbon-containing passivating agent can be any two, any three, or any four combinations of carbon dioxide, low-carbon alkanes, low-carbon olefins, and low-carbon alkynes. Further, the low-carbon alkanes can be alkanes selected from C1-C4, such as at least one of methane, ethane, propane, and butane; the low-carbon olefins can be olefins selected from C2-C4, such as at least one of ethylene, propylene, and butene; and the low-carbon alkynes can be alkynes selected from C2-C4, such as at least one of acetylene, propyne, and butyne.

[0047] Furthermore, the passivating agent is preferably carbon dioxide, methane, or ethylene. In this case, the byproduct methane produced by the sulfidation treatment can be fully utilized. Then, the passivating agent is continued to be introduced. The CO2 in the passivating agent undergoes a reforming reaction, a CO disproportionation reaction, and a CH4 cracking reaction, which is conducive to the aggregation of filamentous carbon between the active metal sites of the catalyst and the catalyst particles.

[0048] According to the technical solution of the present invention, by using a carbon-containing passivating agent that meets the above requirements, carbon deposits can be deposited on the surface of the active metal component of the sulfide-state catalyst. Due to the high dispersion of the active metal component, the passivation treatment helps to alleviate excessive carbon deposition on the catalyst surface, while simultaneously obtaining easily removable α-carbon (filamentous carbon). This carbon deposit protects the active metal sites of the catalyst without causing catalyst deactivation. Specifically, under the temperature conditions of hydrogen and the hydrogenation reaction, the carbon deposits in the hydrogenation catalyst gradually dissolve, promoting the release of active metal sites. Therefore, the hydrogenation catalyst can be directly applied in the hydrogenation process, where the surface carbon decomposes under the conditions of hydrogen and the hydrogenation reaction temperature, allowing the sulfide-state active metal sites of the hydrogenation catalyst to be released again.

[0049] This invention does not limit the specific parameters of the passivation treatment, as long as carbon deposition is formed on the surface of the sulfided catalyst. In one embodiment of this invention, the passivation treatment temperature is 350℃~450℃, for example, 350℃, 370℃, 380℃, 400℃, 410℃, 420℃, 430℃, 450℃ or any combination thereof, and the passivation treatment pressure is 0.5MPa~3.5MPa, for example, preferably 0.5MPa, 1MPa, 1.5MPa, 2MPa, 2.5MPa, 3MPa, 3.5MPa or any combination thereof.

[0050] By properly controlling the amount of carbon-containing passivating agent, the amount of carbon deposited on the surface of the sulfide catalyst can be controlled. In some embodiments, the volume hourly space velocity (HHSV) for passivation treatment is 500 h⁻¹. -1 ~10000h -1 For example, 500h -11000h -1 2000h -1 3000h -1 4000h -1 5000h -1 6000h -1 7000h -1 8000h -1 10000h -1 The passivation time is a range of 2h to 10h, for example, 2h, 4h, 6h, 8h, 10h, or any combination thereof. The volume hourly space velocity (VHSV) refers to the VHSV of the carbon-containing passivating agent, i.e., the volume of carbon-containing passivating agent passing through a unit volume of sulfide-state catalyst per unit time.

[0051] Furthermore, by contacting the sulfide-state hydrogenation catalyst with a mixture of inert gas and carbon-containing passivating agent, the safety of the passivation treatment is ensured. The inert gas includes at least one of helium and nitrogen. While the inert gas does not participate in the reaction, its presence causes a decrease in the partial pressure of the carbon-containing passivating agent in the syngas, thus affecting the reaction rate. Therefore, an appropriate amount of inert gas can be added according to the actual situation. In one embodiment, the volume concentration of the carbon-containing passivating agent in the mixture is 1%-10%, for example, a range of 1%, 2%, 3%, 4%, 5%, 6%, 8%, 10%, or any combination thereof.

[0052] The passivation treatment described above is a gas-solid phase reaction process that can be carried out in reactors such as fluidized beds, fixed beds, spouted beds, and moving beds. For example, a granular sulfide catalyst is packed into a reactor to form a fixed bed of a certain height. A carbon-containing passivating agent is then introduced into the reactor, and passivation is achieved as the carbon-containing passivating agent flows through the fixed bed.

[0053] After the passivation treatment described above, a cooling process is performed under an inert atmosphere until the temperature drops to 0–50°C to obtain the hydrogenation catalyst. The inert atmosphere can be nitrogen.

[0054] This invention does not limit the specific type of metal salt in the metal salt solution during the impregnation process. The metal salt includes, but is not limited to, at least one metallic element from Group VIB and Group VIII of the periodic table. Exemplarily, the metal salt includes at least one of nickel nitrate, nickel acetate, basic nickel carbonate, cobalt nitrate, cobalt acetate, basic cobalt carbonate, ammonium molybdate heptahydrate, ammonium molybdate tetrahydrate, and molybdenum trioxide. The metal salt solution also contains acidic aqueous solutions such as H3PO4, citric acid, and oxalic acid.

[0055] Furthermore, the present invention can prepare hydrorefining catalysts with bimetallic active components. In one embodiment, the metal elements supported on the support in the hydrorefining catalyst include the main active component molybdenum and the co-active components cobalt or nickel, i.e., (molybdenum-nickel catalyst or molybdenum-cobalt catalyst). Based on the hydrorefining catalyst, the total loading of the metals is 10-35 wt%, and further, based on the oxides of the respective metals, the loading of Mo is 5-30 wt%, and the loading of Co or Ni is 1-11 wt%.

[0056] The present invention does not limit the impregnation process. For example, molybdenum salt is placed in an aqueous solution of H3PO4, citric acid, or oxalic acid, and then heated and stirred until the metal salt dissolves. Then, a metal salt containing cobalt or nickel is added, and the pH value of the solution is adjusted to be lower than the zero charge point of the carrier to obtain a metal salt solution. The carrier is impregnated in the metal salt solution using an equal volume saturated impregnation method, left to stand at room temperature for 12-24 hours, and then dried and calcined.

[0057] This invention does not limit the specific parameters for drying and calcination, as long as they enable the metal salt supported on the carrier to form a metal oxide. In one embodiment, the drying conditions are: temperature 80-140℃, time 2-6 hours. The calcination conditions are: temperature 400-700℃, time 4-8 hours. By increasing the calcination temperature, the interaction between the -OH groups on the carrier surface and the metal is strengthened, promoting the dispersion of the active metal component and further improving the dispersion degree of the active metal component.

[0058] This invention also provides a hydrogenation catalyst, prepared using the method described in the first aspect of the invention. This hydrogenation catalyst exhibits excellent performance in terms of safety and catalytic activity, which is beneficial for extending its service life.

[0059] The present invention will be further described below through specific embodiments and comparative examples. Unless otherwise specified, the reagents, materials and instruments used below are all conventional reagents, materials and instruments, all of which are commercially available, and the reagents and materials involved can also be synthesized by conventional synthetic methods.

[0060] In the following examples and comparative examples, the support used was strip-shaped alumina (γ-Al2O3) with a zero charge point of 8.0; the molded catalyst was vulcanized using a temperature-programmed vulcanizer (Tianjin Xianquan, TPS-5096).

[0061] Example 1

[0062] (1) Place 20g of ammonium molybdate in a beaker containing 40mL of deionized water, add 1.5g of phosphoric acid, and then place the beaker in a 50℃ water bath and stir to dissolve for 0.5h; then add 17g of cobalt nitrate, add an appropriate amount of phosphoric acid, adjust the pH of the solution to 3, and stir in a water bath for 0.5h to obtain a metal salt solution; the water absorption rate of the alumina support is 65%, and then use the equal volume saturated impregnation method to load the metal salt solution obtained above onto the support, let it stand and dry for 12h, then dry at 120℃ for 2h, and calcine at 400℃ for 4h to obtain the CoMo / Al2O3 catalyst;

[0063] (2) Measure 100 mL of 20-40 mesh CoMo / Al2O3 catalyst and fill it into the reactor. Purge the reactor with nitrogen for 2 h. When the temperature is raised to 160℃, carbon disulfide and hydrogen are introduced for sulfidation treatment to obtain the sulfidated catalyst. The sulfidation treatment conditions are as follows: the amount of carbon disulfide injected is based on the volume fraction of hydrogen sulfide in the reactor reaching 3.0%, the temperature is 320℃, the pressure is 0.5MPa, and the sulfidation time is 6 h.

[0064] (3) After the sulfidation treatment, a mixture of inert gas and carbon-containing passivating agent is introduced into the reactor to passivate the sulfidated catalyst. The carbon-containing passivating agent is methane and carbon dioxide (volume ratio of 60:40). The concentration of the carbon-containing passivating agent in the mixture is 8v%. The passivation conditions are: temperature 360℃, pressure 2.0MPa, and volume hourly space velocity 8000h. -1 The time was 6 hours; the reactor was heated at a rate of 20℃ / h.

[0065] (4) After passivation, nitrogen gas is introduced into the reactor. When the temperature drops to 30°C, the passivated CoMo / Al2O3 catalyst is unloaded and named C1.

[0066] Example 2

[0067] (1) Place 20g of ammonium molybdate in a beaker containing 40mL of deionized water, add 1.5g of citric acid, and then place the beaker in a 50℃ water bath and stir to dissolve for 0.5h; then add 17g of cobalt nitrate, and add an appropriate amount of citric acid to adjust the pH of the solution to 4.0, and stir in a water bath for 0.5h to obtain a metal salt solution; wherein the water absorption rate of the alumina support is 65%, and then use the equal volume saturated impregnation method to load the metal salt solution obtained above onto the support, let it stand and dry for 12h, then dry at 120℃ for 2h, and calcine at 450℃ for 4h to obtain the CoMo / Al2O3 catalyst;

[0068] (2) Measure 100 mL of 20-40 mesh CoMo / Al2O3 catalyst and fill it into the reactor. Purge the reactor with nitrogen for 2 h. When the temperature is raised to 160℃, thiol and hydrogen are introduced for sulfidation treatment to obtain sulfidated catalyst. The conditions for sulfidation treatment are: the amount of thiol injected is based on the volume fraction of hydrogen sulfide in the reactor reaching 3.0%, the temperature is 320℃, the pressure is 0.5MPa, and the sulfidation time is 6 h.

[0069] (3) After the sulfidation treatment, a mixture of inert gas and carbon-containing passivating agent is introduced into the reactor to passivate the sulfidated catalyst. The carbon-containing passivating agent consists of methane, carbon dioxide, and ethylene (volume ratio of 40:40:20). The concentration of the carbon-containing passivating agent in the mixture is 8v%. The passivation conditions are: temperature 360℃, pressure 2.0MPa, and volume hourly space velocity 8000h. -1 The time was 6 hours; the reactor was heated at a rate of 20℃ / h.

[0070] (4) After passivation, nitrogen gas is introduced into the reactor. When the temperature drops to 30°C, the passivated CoMo / Al2O3 catalyst is unloaded and named C2.

[0071] Example 3

[0072] (1) Place 20g of ammonium molybdate in a beaker containing 40mL of deionized water, add 1.5g of oxalic acid, and then place the beaker in a 50℃ water bath and stir to dissolve for 0.5h; then add 17g of basic cobalt carbonate, add an appropriate amount of oxalic acid, adjust the pH of the solution to 3.5, and stir in a water bath for 0.5h to obtain a metal salt solution; wherein, the water absorption rate of the alumina support is 65%, and then use the equal volume saturated impregnation method to load the metal salt solution obtained above onto the support, let it stand and dry for 12h, then dry at 120℃ for 2h, and calcine at 500℃ for 4h to obtain the CoMo / Al2O3 catalyst;

[0073] (2) Measure 100 mL of 20-40 mesh CoMo / Al2O3 catalyst and fill it into the reactor. Purge the reactor with nitrogen for 2 hours. When the temperature is raised to 160℃, introduce dimethyl sulfide and hydrogen for sulfidation. The sulfidation conditions are: the amount of dimethyl sulfide injected is based on the volume fraction of hydrogen sulfide in the reactor reaching 3.0%, the temperature is 320℃, the pressure is 0.5MPa, and the sulfidation time is 6 hours.

[0074] (3) After the sulfidation treatment, a mixture of inert gas and carbon-containing passivating agent is introduced into the reactor to passivate the sulfidated catalyst. The carbon-containing passivating agent is methane and ethylene (volume ratio of 70:30). The concentration of the carbon-containing passivating agent in the mixture is 8v%. The passivation conditions are: temperature 360℃, pressure 2.0MPa, and volume hourly space velocity 8000h. -1 The time was 6 hours; the reactor was heated at a rate of 20℃ / h.

[0075] (4) After passivation, nitrogen gas is introduced into the reactor. When the temperature drops to 30°C, the passivated sulfide CoMo / Al2O3 catalyst is unloaded and named C3.

[0076] Example 4

[0077] (1) Place 20g of ammonium molybdate in a beaker containing 40mL of deionized water, add 1.5g of phosphoric acid, and then place the beaker in a 50℃ water bath and stir to dissolve for 0.5h; then add 17g of cobalt acetate, and add an appropriate amount of phosphoric acid to adjust the pH of the solution to 2.0, and stir in a water bath for 0.5h to obtain a metal salt solution; wherein the water absorption rate of the alumina support is 65%, and then use the equal volume saturated impregnation method to load the metal salt solution obtained above onto the support, let it stand and dry for 12h, then dry at 120℃ for 2h, and calcine at 550℃ for 4h to obtain the CoMo / Al2O3 catalyst;

[0078] (2) Measure 100 mL of 20-40 mesh CoMo / Al2O3 catalyst and fill it into the reactor. Purge the reactor with nitrogen for 2 hours. When the temperature is raised to 160℃, introduce carbon disulfide, mercaptan and hydrogen to sulfide to obtain the sulfided catalyst. The sulfidation conditions are as follows: the injection amount of carbon disulfide and mercaptan (volume ratio of the two is 50:50) is based on the hydrogen sulfide volume fraction in the reactor reaching 3.0%, the temperature is 320℃, the pressure is 0.5MPa, and the sulfidation time is 6 hours.

[0079] (3) After the sulfidation treatment, a mixture of inert gas and carbon-containing passivating agent is introduced into the reactor to passivate the sulfidated catalyst. The carbon-containing passivating agent consists of methane, carbon dioxide, and propylene (volume ratio of 40:40:20). The concentration of the carbon-containing passivating agent in the mixture is 8v%. The passivation conditions are: temperature 360℃, pressure 2.0MPa, and volume hourly space velocity 8000h. -1 The time was 6 hours; the reactor was heated at a rate of 20℃ / h.

[0080] (4) After passivation, nitrogen gas is introduced into the reactor. When the temperature drops to 30°C, the passivated CoMo / Al2O3 catalyst is unloaded and named C4.

[0081] Example 5

[0082] (1) Place 20g of ammonium molybdate in a beaker containing 40mL of deionized water, add 1.5g of phosphoric acid, and then place the beaker in a 50℃ water bath and stir to dissolve for 0.5h; then add 17g of cobalt nitrate, add an appropriate amount of phosphoric acid, adjust the pH of the solution to 4.0, and stir in a water bath for 0.5h to obtain a metal salt solution; wherein, the water absorption rate of the alumina support is 65%, and then use the equal volume saturated impregnation method to load the metal salt solution obtained above onto the support, let it stand and dry for 12h, then dry at 120℃ for 2h, and calcine at 600℃ for 4h to obtain the CoMo / Al2O3 catalyst;

[0083] (2) Measure 100 ml of 20-40 mesh CoMo / Al2O3 catalyst, fill it into the reactor, purge the reactor with nitrogen for 2 h, and when the temperature is raised to 160℃, introduce carbon disulfide, dimethyl sulfide and hydrogen to sulfide to obtain the sulfided catalyst; the sulfidation conditions are: the injection amount of carbon disulfide and dimethyl sulfide (the volume ratio of the two is 50:50) is based on the hydrogen sulfide volume fraction in the reactor reaching 3.0%, the temperature is 320℃, the pressure is 0.5MPa, and the sulfidation time is 6 h;

[0084] (3) After the sulfidation treatment, a mixture of inert gas and carbon-containing passivating agent is introduced into the reactor to passivate the sulfidated catalyst. The carbon-containing passivating agent is ethane, carbon dioxide, and ethylene (volume ratio of 40:40:20). The concentration of the carbon-containing passivating agent in the mixture is 8v%. The passivation conditions are: temperature 360℃, pressure 2.0MPa, and volume hourly space velocity 8000h. -1 The time was 6 hours; the reactor was heated at a rate of 20℃ / h.

[0085] (4) After passivation, nitrogen gas is introduced into the reactor. When the temperature drops to 30°C, the passivated CoMo / Al2O3 catalyst is unloaded and named C5.

[0086] Example 6

[0087] (1) Place 20g of ammonium molybdate in a beaker containing 40mL of deionized water, add 1.5g of phosphoric acid, and then place the beaker in a 50℃ water bath and stir to dissolve for 0.5h; then add 17g of cobalt nitrate, and add an appropriate amount of phosphoric acid to adjust the pH of the solution to 4.0, and stir in a water bath for 0.5h to obtain a metal salt solution; wherein the water absorption rate of the alumina support is 65%, and then use the equal volume saturated impregnation method to load the metal salt solution obtained above onto the support, let it stand and dry for 12h, then dry at 120℃ for 2h, and calcine at 650℃ for 4h to obtain the CoMo / Al2O3 catalyst;

[0088] (2) Measure 100 mL of 20-40 mesh CoMo / Al2O3 catalyst and fill it into the reactor. Purge the reactor with nitrogen for 2 h. When the temperature is raised to 160℃, introduce dimethyl disulfide and hydrogen to sulfide to obtain the sulfided catalyst. The sulfidation conditions are as follows: the amount of dimethyl disulfide injected is based on the volume fraction of hydrogen sulfide in the reactor of 3.0%, the temperature is 320℃, the pressure is 0.5MPa, and the sulfidation time is 6 h.

[0089] (3) After the sulfidation treatment, a mixture of inert gas and carbon-containing passivating agent is introduced into the reactor to passivate the sulfidated catalyst. The carbon-containing passivating agent consists of methane, carbon dioxide, and ethylene (volume ratio of 50:30:20). The concentration of the carbon-containing passivating agent in the mixture is 8v%. The passivation conditions are: temperature 360℃, pressure 2.0MPa, and volume hourly space velocity (VHSV) 8000h. -1 The time was 6 hours; the reactor was heated at a rate of 20℃ / h.

[0090] (4) After passivation, nitrogen gas is introduced into the reactor. When the temperature drops to 30°C, the passivated CoMo / Al2O3 catalyst is unloaded and named C6.

[0091] Example 7

[0092] (1) Place 20g of ammonium molybdate in a beaker containing 40mL of deionized water, add 1.5g of phosphoric acid, and then place the beaker in a 50℃ water bath and stir to dissolve for 0.5h; then add 17g of cobalt acetate, and add an appropriate amount of phosphoric acid to adjust the pH of the solution to 4.0, and stir in a water bath for 0.5h to obtain a metal salt solution; wherein the water absorption rate of the alumina support is 65%, and then use the equal volume saturated impregnation method to load the metal salt solution obtained above onto the support, let it stand and dry for 12h, then dry at 120℃ for 2h, and calcine at 700℃ for 4h to obtain the CoMo / Al2O3 catalyst;

[0093] (2) Measure 100 mL of 20-40 mesh CoMo / Al2O3 catalyst and fill it into the reactor. Purge the reactor with nitrogen for 2 hours. When the temperature is raised to 160℃, carbon disulfide, dimethyl sulfide and hydrogen are introduced for sulfidation to obtain the sulfidated catalyst. The sulfidation conditions are as follows: the injection amount of carbon disulfide and dimethyl sulfide (volume ratio of the two is 50:50) is based on the volume fraction of hydrogen sulfide in the reactor being 3.0%, the temperature is 320℃, the pressure is 0.5MPa, and the sulfidation time is 6 hours.

[0094] (3) After sulfidation, a mixture of inert gas and carbon-containing passivating agent is introduced into the reactor to passivate the sulfidated catalyst. The carbon-containing passivating agent is methane and propylene (volume ratio of 60:40). The concentration of the carbon-containing passivating agent in the mixture is 8v%. The passivation conditions are: temperature 360℃, pressure 2.0MPa, and volume hourly space velocity 8000h. -1 The time was 6 hours; the reactor was heated at a rate of 20℃ / h.

[0095] (4) After passivation, nitrogen gas is introduced into the reactor. When the temperature drops to 30°C, the passivated CoMo / Al2O3 catalyst is unloaded and named C7.

[0096] Example 8

[0097] (1) Place 20g of ammonium molybdate in a beaker containing 40mL of deionized water, add 1.5g of phosphoric acid, and then place the beaker in a 50℃ water bath and stir to dissolve for 0.5h; then add 17g of nickel nitrate, and then add an appropriate amount of phosphoric acid to adjust the pH of the solution to 3.0, and stir in a water bath for 0.5h to obtain a metal salt solution; wherein the water absorption rate of the alumina support is 65%, and then use the equal volume saturated impregnation method to load the metal salt solution prepared above onto the support, let it stand and dry for 12h, then dry at 120℃ for 2h, and calcine at 650℃ for 4h to obtain NiMo / Al2O3 catalyst;

[0098] (2) Measure 100 mL of 20-40 mesh NiMo / Al2O3 catalyst and fill it into the reactor. Purge the reactor with nitrogen for 2 h. When the temperature is raised to 160℃, introduce carbon disulfide, mercaptan, dimethyl sulfide and hydrogen to sulfide to obtain the sulfided catalyst. The sulfidation conditions are as follows: the volume ratio of carbon disulfide, mercaptan and dimethyl sulfide is 40:30:30. The injection amount is based on the volume fraction of hydrogen sulfide in the reactor of 3.0%. The temperature is 320℃, the pressure is 0.5MPa and the sulfidation time is 6 h.

[0099] (3) After the sulfidation treatment, a mixture of inert gas and carbon-containing passivating agent is introduced into the reactor to passivate the sulfidated catalyst. The carbon-containing passivating agent is methane, ethylene, and acetylene (volume ratio of 70:20:10). The concentration of the carbon-containing passivating agent in the mixture is 8v%. The passivation conditions are: temperature 360℃, pressure 2.0MPa, and volume hourly space velocity 8000h. -1 The time was 6 hours; the reactor was heated at a rate of 20℃ / h.

[0100] (4) After passivation, nitrogen gas is introduced into the reactor. When the temperature drops to 30°C, the passivated NiMo / Al2O3 catalyst is unloaded and named C8.

[0101] Example 9

[0102] (1) Place 20g of ammonium molybdate in a beaker containing 40mL of deionized water, add 1.5g of acetic acid, and then place the beaker in a 50℃ water bath and stir for 0.5h to completely dissolve the molybdenum salt; then add 17g of nickel acetate, and then add an appropriate amount of acetic acid to adjust the pH of the solution to 4.0, and stir in a water bath for 0.5h to obtain a metal solution; wherein the water absorption rate of the alumina support is 65%, and then use the equal volume saturated impregnation method to load the metal salt solution prepared above onto the support, let it stand and dry for 12h, then dry at 120℃ for 2h, and calcine at 600℃ for 4h to obtain NiMo / Al2O3 catalyst;

[0103] (2) Measure 100 mL of 20-40 mesh NiMo / Al2O3 catalyst and fill it into the reactor. Purge the reactor with nitrogen for 2 h. When the temperature is raised to 160℃, carbon disulfide and hydrogen are introduced for sulfidation to obtain the sulfidated catalyst. The sulfidation conditions are as follows: the amount of carbon disulfide injected is based on the volume fraction of hydrogen sulfide in the reactor of 3.0%, the temperature is 320℃, the pressure is 0.5MPa, and the sulfidation time is 6 h.

[0104] (3) After sulfidation, a mixture of inert gas and carbon-containing passivating agent is introduced into the reactor to passivate the sulfidated catalyst. The carbon-containing passivating agent is carbon dioxide and ethylene (volume ratio of 50:50). The concentration of the carbon-containing passivating agent in the mixture is 8v%. The passivation conditions are: temperature 360℃, pressure 2.0MPa, and volume hourly space velocity 8000h. -1 The time was 6 hours; the reactor was heated at a rate of 20℃ / h.

[0105] (4) After passivation, nitrogen gas is introduced into the reactor. When the temperature drops to 30°C, the passivated NiMo / Al2O3 catalyst is unloaded and named C9.

[0106] Example 10

[0107] (1) Place 20g of ammonium molybdate in a beaker containing 40mL of deionized water, add 1.5g of phosphoric acid, and then place the beaker in a 50℃ water bath and stir to dissolve for 0.5h; then add 17g of basic nickel carbonate, and add an appropriate amount of phosphoric acid to adjust the pH of the solution to 4.0, and stir in a water bath for 0.5h to obtain a metal salt solution; wherein the water absorption rate of the alumina support is 65%, and then use the equal volume saturated impregnation method to load the metal salt solution obtained above onto the support, let it stand and dry for 12h, then dry at 120℃ for 2h, and calcine at 650℃ for 4h to obtain NiMo / Al2O3 catalyst;

[0108] (2) Measure 100 mL of 20-40 mesh NiMo / Al2O3 catalyst and fill it into the reactor. Purge the reactor with nitrogen for 2 h. When the temperature is raised to 160℃, carbon disulfide and hydrogen are introduced for sulfidation to obtain the sulfidated catalyst. The sulfidation conditions are as follows: the amount of carbon disulfide injected is based on the volume fraction of hydrogen sulfide in the reactor of 3.0%, the temperature is 320℃, the pressure is 0.5MPa, and the sulfidation time is 6 h.

[0109] (3) After sulfidation, a mixture of inert gas and carbon-containing passivating agent is introduced into the reactor to passivate the sulfidated catalyst. The carbon-containing passivating agent is methane and propyne (volume ratio of 70:30). The concentration of the carbon-containing passivating agent in the mixture is 8v%. The passivation conditions are: temperature 360℃, pressure 2.0MPa, and volume hourly space velocity 8000h. -1 The time was 6 hours; the reactor was heated at a rate of 20℃ / h.

[0110] (4) After passivation, nitrogen gas is introduced into the reactor. When the temperature drops to 30°C, the passivated NiMo / Al2O3 catalyst is unloaded and named C10.

[0111] Comparative Example 1

[0112] (1) Place 20g of ammonium molybdate in a beaker containing 20mL of deionized water, then add 20g of 0.1mol / L ammonia water to adjust the pH of the solution to 10.0. Then place the beaker in a 30℃ water bath and stir to dissolve for 15 minutes. After that, add 17g of cobalt nitrate and stir in a water bath for 0.5h to obtain a metal salt solution. The water absorption rate of the alumina support strip is calculated to be 65%. Then, the metal salt solution prepared above is loaded onto the support by the equal volume saturated impregnation method, and allowed to stand and dry for 12h. Then, it is dried at 120℃ for 2h and calcined at 400℃ for 4h to obtain the CoMo / Al2O3 catalyst.

[0113] (2) Measure 100 mL of 20-40 mesh CoMo / Al2O3 catalyst and fill it into the reactor. Purge the reactor with nitrogen for 2 h. When the temperature is raised to 160℃, carbon disulfide and hydrogen are introduced for sulfidation to obtain the sulfidated catalyst. The sulfidation conditions are as follows: the amount of carbon disulfide injected is based on the volume fraction of hydrogen sulfide in the reactor of 3.0%, the temperature is 320℃, the pressure is 0.5MPa, and the sulfidation time is 6 h.

[0114] (3) After sulfidation, a mixture of inert gas and carbon-containing passivating agent is introduced into the reactor to passivate the sulfidated catalyst. The carbon-containing passivating agent consists of methane, carbon dioxide, and ethylene (volume ratio of 40:40:20). The concentration of the carbon-containing passivating agent in the mixture is 8v%. The passivation conditions are: temperature 360℃, pressure 2.0MPa, and volume hourly space velocity (VHSV) 8000h. -1 The time was 6 hours; the reactor was heated at a rate of 20℃ / h.

[0115] (4) After passivation, nitrogen gas is introduced into the reactor. When the temperature drops to 30°C, the passivated CoMo / Al2O3 catalyst is unloaded and named D1.

[0116] Comparative Example 2

[0117] (1) Place 20g of ammonium molybdate in a beaker containing 40mL of deionized water, add 1.5g of phosphoric acid, and then place the beaker in a 50℃ water bath and stir for 0.5h to completely dissolve the molybdenum salt; then add 17g of cobalt nitrate and stir in a water bath for 0.5h to obtain a metal salt solution with a pH of 6.2; the water absorption rate of the alumina support strip is 65%, and then the metal salt solution prepared above is loaded onto the support by the equal volume saturated impregnation method, allowed to stand and dry for 12h, then dried at 120℃ for 2h, and calcined at 400℃ for 4h to obtain the CoMo / Al2O3 catalyst;

[0118] (2) Measure 100 mL of 20-40 mesh CoMo / Al2O3 catalyst and fill it into the reactor. Purge the reactor with nitrogen for 2 h. When the temperature is raised to 160℃, carbon disulfide and hydrogen are introduced for sulfidation to obtain the sulfidated catalyst. The sulfidation conditions are as follows: the amount of carbon disulfide injected is based on the volume fraction of hydrogen sulfide in the reactor of 3.0%, the temperature is 320℃, the pressure is 0.5MPa, and the sulfidation time is 6 h.

[0119] (3) After sulfidation, an oxygen-containing passivating agent is introduced into the reactor to passivate the sulfidated catalyst. The oxygen-containing passivating agent is a 2.0 v% O2 / N2 mixed gas. The passivation conditions are: temperature 360℃, pressure 2.0 MPa, and volume hourly space velocity 8000 h⁻¹. -1 The time was 6 hours; the reactor was heated at a rate of 20℃ / h.

[0120] (4) After passivation, nitrogen gas is introduced into the reactor. When the temperature drops to 30°C, the passivated CoMo / Al2O3 catalyst is unloaded and named D2.

[0121] Test case

[0122] 1. Passivation effect

[0123] Weigh 0.15g to 0.2g of hydrogenation catalyst and use a high-frequency infrared carbon-sulfur analyzer (Leco CS744) to detect the sulfur and carbon content on its surface;

[0124] Calculate the sulfur retention rate (%) and carbon deposition rate (%) using the following formulas:

[0125] C(%)=100×(G / m)×Fdrift

[0126] Where G: mass of the element being analyzed (g)

[0127] m: Sample mass (g)

[0128] Fdrift is the coefficient value for adjusting instrument drift.

[0129] 2. Hydrogenation activity

[0130] Hydrodesulfurization: The hydrodesulfurization activity of the hydrocatalysts in the examples and comparative examples was evaluated using FCC gasoline with a sulfur content of 100 ppm to 125 ppm and an olefin content of 20% to 24% as feedstock. The reaction conditions were: temperature 280°C, pressure 2.0 MPa, and space velocity 2.5 h⁻¹. -1 With a hydrogen-to-oil ratio of 300:1, samples were taken after the reaction stabilized for 48 hours to determine the sulfur and olefin content in the reaction products. The sulfur content in the oil was determined using a sulfur-nitrogen analyzer (analytikjena multiEA 5000) to verify the hydrodesulfurization performance of the hydrotreating catalyst. PONA analysis was used to determine the group composition and to detect the olefin saturation degree of the hydrotreating catalyst, i.e., the hydrotreating saturation. The hydrotreating saturation degree is related to the octane number loss in gasoline products; the higher the hydrotreating saturation degree, the greater the octane number loss.

[0131] The test results are shown in Table 1;

[0132] The formulas for calculating hydrodesulfurization activity and hydrogen saturation rate are as follows:

[0133]

[0134]

[0135] 3. The morphology of the carbon deposits was observed using a Japanese transmission electron microscope (TEM) 2100plus. The test results are shown in [see attached image]. Figure 2 .

[0136] 4. Analysis of Carbon Deposition Types in H2-TPR (H2 Temperature Programmed Reduction)

[0137] The distribution and content of carbon deposits in the hydrogenation catalyst were detected using H2-TPR, and the test results are shown in Table 3.

[0138] Table 1

[0139]

[0140]

[0141] In the table, "-" indicates no data.

[0142] Table 2

[0143]

[0144] As shown in Table 1, this invention successfully prepared a shaped catalyst with high metal loading and high dispersion by adjusting the pH value of the impregnation solution and the calcination temperature. Compared with the catalyst prepared without adjusting the pH value of the metal salt solution, it exhibits superior hydrodesulfurization activity. Simultaneously, carbon dioxide, methane, and ethylene were selected as passivating agents in the passivation treatment. Due to the high dispersion of the active metal on the support surface, this helps to alleviate excessive carbon deposition on the catalyst surface and promotes the aggregation of active centers and catalyst particles to form α-carbon (filamentous carbon), such as... Figure 2 As shown in (d), α-carbon can selectively coat the active sites, which are completely decomposed by hydrogen as the reaction temperature increases during the start-up process, promoting the release of hydrogenated active sites.

[0145] according to Figure 3 As shown in Table 2, the hydrogenation catalyst provided by the present invention can effectively control the type of carbon deposit and obtain the target product, filamentous carbon. In contrast, the carbon deposits obtained in the comparative example are graphitic carbon and spherical coated carbon. These two types of carbon cannot be decomposed by hydrogen during the hydrogenation reaction (reaction temperature < 380°C), resulting in the inability to release the covered hydrogenation active sites and affecting the catalytic activity of the catalyst.

[0146] The preferred embodiments and experimental verifications of the present invention have been described in detail above. It should be understood that those skilled in the art can make numerous modifications and variations based on the concept of the present invention without creative effort. Therefore, all technical solutions that can be obtained by those skilled in the art based on the concept of the present invention through logical analysis, reasoning, or limited experimentation on the basis of existing technology should be within the scope of protection defined by the claims.

Claims

1. A method for preparing a hydrogenation catalyst, characterized in that, Includes the following steps: A shaped catalyst is obtained by impregnating a support with a metal salt solution, followed by drying and calcination; wherein the pH value of the metal salt solution is lower than the zero point of charge of the support. The shaped catalyst is subjected to sulfidation treatment to obtain a sulfidated catalyst; A hydrogenation catalyst was obtained by passivating a sulfidated catalyst with a carbon-containing passivating agent. The passivation treatment is performed by contacting the sulfidated catalyst with a mixture of an inert gas and a carbon-containing passivating agent; the carbon-containing passivating agent is selected from at least two of carbon dioxide, C1-C4 alkanes, C2-C4 alkenes, and C2-C4 alkynes. The passivation treatment conditions are: temperature 350℃~450℃, pressure 0.5 MPa~3.5 MPa, and volume hourly space velocity 500 h⁻¹. -1 ~10000h -1 Time: 2 hours to 10 hours; The carbon deposit type of the hydrogenation catalyst is filamentous carbon.

2. The preparation method according to claim 1, characterized in that, The zero point of the carrier is obtained by a method comprising the following steps: mixing the carrier with deionized water to form a suspension of 0.4 g / L, and adjusting the pH of the suspension to bring the zeta potential of the suspension to zero. When the zeta potential of the suspension reaches zero, the pH value of the suspension is the zero electrical point of the carrier.

3. The preparation method according to claim 1, characterized in that, The molding catalyst is subjected to the sulfidation treatment under the combined action of a sulfiding agent and hydrogen; wherein the sulfiding agent includes at least one of hydrogen sulfide, mercaptan, carbon disulfide, dimethyl sulfide, dimethyl disulfide, and phenyl thio compounds.

4. The preparation method according to claim 3, characterized in that, The conditions for the vulcanization treatment are: temperature of 200-400℃, pressure of 0.1-3.0MPa, and time of 2-20h.

5. The preparation method according to claim 3, characterized in that, In the mixed gas, the volume concentration of the carbon passivating agent is 1%-10%.

6. The preparation method according to any one of claims 1-5, characterized in that, The metal salt solution includes at least one metallic element from Group VIB and Group VIII of the periodic table.

7. The preparation method according to any one of claims 1-5, characterized in that, The drying conditions are: temperature 80-140℃, time 2-6 hours; and / or, The calcination conditions are: temperature 400-700℃, time 4-8h.

8. A hydrogenation catalyst, characterized in that, It is prepared by the preparation method according to any one of claims 1-5.

Citation Information

Patent Citations

  • Preparation method of hydrodesulfurization catalyst

    CN108236958A

  • Pre-sulfurization method of heavy oil hydrogenation catalyst and heavy oil hydrogenation pre-sulfurization catalyst

    CN113908888A