Silver-europium co-activated spectral conversion microphase glass and preparation method thereof

By using silver-europium co-doped glass to absorb ultraviolet photons and convert them into visible photons, the problem of poor stability of perovskite solar cells under ultraviolet irradiation is solved, and the photoelectric conversion efficiency and ultraviolet photon utilization rate are improved.

CN118206280BActive Publication Date: 2026-11-24ZHEJIANG UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410254840.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-06
Publication Date
2026-11-24
Estimated Expiration
2044-03-06

AI Technical Summary

Technical Problem

Existing organic-inorganic hybrid perovskite solar cells exhibit poor stability under ultraviolet irradiation and low ultraviolet photon utilization, which affects photoelectric conversion efficiency.

Method used

By introducing silver and europium co-doping into the glass, boron-rich and fluorine-rich phases are formed. Silver exists in the forms of Ag⁺ and Ag⁰, and europium exists in the forms of Eu²⁺ and Eu³⁺. By utilizing the oxidizing properties of Ag⁺ and the luminescent properties of Eu³⁺, ultraviolet photons are absorbed and converted into visible photons, thus preventing the degradation of active materials by ultraviolet photons.

Benefits of technology

This improves the stability and visible photon utilization of perovskite solar cells under ultraviolet irradiation, enhances photoelectric conversion efficiency, and the glass exhibits high ultraviolet absorption, broad-spectrum fluorescence characteristics, and high visible transmittance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118206280B_ABST
    Figure CN118206280B_ABST
Patent Text Reader

Abstract

This invention discloses a silver-europium co-activated spectral conversion differential phase glass and its preparation method. The glass comprises a boron-rich phase and a fluorine-rich phase, with the silver-doped boron-rich phase comprising 60-75% and the europium-doped fluorine-rich phase comprising 25-40% by mass percentage. The boron-rich phase has the following elemental composition by mass percentage: O (35-45%), B (8-20%), Al (5-16%), Ba (4-14%), and Ag (25-35%). The fluorine-rich phase has the following elemental composition by mass percentage: F (15-30%), Ba (65%-84%), and Eu (0.5-10%). The glass is prepared using a three-step method: high-temperature melting, shaping, and low-temperature annealing. The glass prepared by this invention has excellent properties such as large absorption coefficient in the ultraviolet band, high broadband fluorescence efficiency in the red band, and stable physicochemical properties. It can be made into sheet glass and used as an anti-ultraviolet radiation layer and spectral conversion material for perovskite solar cells. It is used to modulate ultraviolet light in the solar spectrum into visible light, which can effectively solve the problems of poor ultraviolet radiation resistance and low utilization rate in the ultraviolet region of perovskite solar cells, thereby improving the photoelectric conversion efficiency of perovskite solar cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a differential phase glass co-doped with noble metals and rare earth elements and its preparation method, and more particularly to a silver-europium co-activated spectral conversion differential phase glass and its preparation method. Background Technology

[0002] Organic-inorganic hybrid perovskite solar cells have shown great promise in both terrestrial and space photovoltaic fields due to their superior photovoltaic performance, excellent power-to-weight ratio, and cost-effectiveness. Their photoelectric conversion efficiency has reached 25.5%, comparable to silicon-based solar cells. However, their poor environmental stability, easily affected by humidity, oxygen, temperature, and light, limits their industrial application. For example, commonly used lead methylammonium iodide (CH3NH3PbI3, or MAPbI3) has a band gap of 1.56–1.70 eV and can absorb photons with wavelengths of 729–785 nm. However, the visible light wavelength of the full solar spectrum is between 400–760 nm, accounting for 50% of the total energy, while ultraviolet light is between 100–400 nm, accounting for only 7%, with the remainder being infrared light >760 nm. These solar cells have a low probability of absorbing infrared light, but near-infrared irradiation can improve the performance of solar cell devices to some extent. Numerous experiments have shown that ultraviolet (UV) irradiation has a significant destructive effect on organic-inorganic hybrid perovskite solar cells. UV light can be divided into UVA (315–400 nm), UVB (280–315 nm), and UVC (100–280 nm) based on wavelength, with UVA accounting for approximately 98.1%, UVB for 1.1%, and UVC being extremely rare. Studies have shown that when MAPbI3-based perovskite solar cell devices are irradiated with UVA, most of the UV light is absorbed by the electron transport layer, exciting electron-hole pairs. This generates a large number of energy level defects at the interface between the electron transport layer and MAPbI3, leading to the accumulation of holes and oxidation of the perovskite layer, accelerating its decomposition and causing rapid degradation of cell performance. Therefore, UV radiation is one of the main factors affecting the stability of perovskite solar cells. Improving the photoelectric conversion efficiency of perovskite solar cells hinges on enhancing their stability under UV irradiation and the utilization rate of the UV band of the solar spectrum.

[0003] In inorganic glasses, silver exists in three forms: silver ions (Ag) + ), silver quantum clusters ([Ag) m ] n+ ) and silver nanoparticles (Ag NPs). [Ag m ] n+ With a charge n, ranging from a few to hundreds of Ag + and silver atoms (Ag) 0 Composed of n Ag, it can be viewed as n Ag units. + and (mn) Ag 0Formed by aggregation, with dimensions at the nanometer level. [Ag] m ] n+ The electronic energy levels are not continuous; transitions between energy levels can produce strong ultraviolet light absorption and visible light emission, exhibiting advantages such as broad-spectrum fluorescence and high efficiency. [Ag] m ] n+ In contrast, Ag NPs are mainly composed of Ag 0 It has a lower charge, higher degree of polymerization, and larger size, but it does not produce fluorescence emission. Instead, it undergoes surface plasmon resonance (SPR) in the blue-green wavelength range, thus affecting the efficient fluorescence emission and visible transmittance of inorganic glasses in the visible light band. Cationic B 3+ Al 3+ and Ba 2+ It will form negatively charged tetrahedrons [BO4] in the glass. - [AlO4] - and [BaO4] 2- This can suppress excessive reduction of silver, reducing the likelihood of silver nanoparticle formation and thus achieving optical stability of silver. Europium in glass generally exists as divalent europium ions (Eu). 2+ ) and trivalent europium ions (Eu) 3+ The structure of inorganic glasses containing EuF3 exists in the form of a network exosome with a high coordination number, resulting in a relatively compact structure. Introducing an appropriate amount of EuF3 into the glass can enhance its chemical stability, which is related to aluminum ions (Al2O3). 3+ The effect of europium on glass modification is similar. However, if excessive europium is introduced, it will react with Ag, which also acts as a network exogenous substance. + Competition for positions, thereby promoting Ag + Reduced to silver atoms (Ag) 0 This increases the likelihood of forming silver nanoparticles (Ag NPs). Therefore, introducing europium can increase the density of the network structure, but it may also reduce the density of Ag. + Solubility. Eu 2+ The luminescence is caused by fd transitions, and the luminescence characteristics are ultraviolet excitation and visible emission; Eu 3+ The luminescence occurs via an ff transition, characterized by excitation with violet-blue light and emission with red-orange light. Doping the glass with both silver and europium luminescent centers can not only appropriately improve the glass's physicochemical stability but also potentially broaden the excitation and emission wavelengths. Compared to ordinary transparent silver borate glass, which absorbs photons in the UVB and UVC regions through Ag but has poor absorption in the 98.1% UVA region, using Eu... 2+ Absorbing UVA photons enhances the glass's ability to absorb ultraviolet photons, thus improving the stability of perovskite solar cells under ultraviolet irradiation. Simultaneously, through Eu... 3+The red-orange light emission of Ag / Eu can further improve the device performance of perovskite solar cells. However, Ag / Eu co-doping creates redox ion pairs, one reducing and the other oxidizing. Therefore, one strategy is to enrich the two in different regions, i.e., Ag in the boron-rich phase and Eu in the fluorine-rich phase. Introducing a small amount of fluorine can also improve the visible light transmittance of the glass. Introducing alkaline earth metal ions into the glass can, on the one hand, form a large number of negatively charged polyhedra to suppress the excessive reduction of silver, and on the other hand, achieve a uniform glass structure and obtain extremely small phase separation. Therefore, using silver-europium co-doped boron-barium-aluminum oxide network inorganic glass as the spectral conversion material of the UV-resistant layer of perovskite solar cells can effectively absorb ultraviolet photons and prevent the degradation of active materials by ultraviolet photons; using [Ag m ] n+ The broad-spectrum fluorescence properties of europium ions convert ultraviolet photons into visible photons, improving the perovskite solar cell's resistance to ultraviolet radiation damage and increasing the utilization rate of visible photons, thereby further enhancing the photoelectric conversion efficiency of perovskite solar cells. Summary of the Invention

[0004] The purpose of this invention is to address the shortcomings of existing technologies by providing a silver europium co-activated spectral conversion differential phase glass and its preparation method.

[0005] In a first aspect, embodiments of the present invention provide a silver-europium co-activated spectral conversion differential phase glass, wherein the silver-europium co-activated spectral conversion differential phase glass contains a boron-rich phase and a fluorine-rich phase, and has the following composition by mass percentage:

[0006] Silver-doped boron-rich phase: 60–75%;

[0007] Europium-doped fluorine-rich phase: 25-40%.

[0008] Furthermore, the silver-doped boron-rich phase has the following elemental composition by mass percentage:

[0009]

[0010] Furthermore, the europium-doped fluorine-rich phase has the following elemental composition by mass percentage:

[0011] F 15~30%;

[0012] Ba 65%–84%;

[0013] Eu 0.5–10%.

[0014] Furthermore, in the silver-doped boron-rich phase of the silver-europium co-activated spectral conversion differential phase glass, Ag is in the +1 valence phase. + Ions and Ag with zero oxidation state 0They exist in atomic form, and the total content of Ag in both forms is as follows:

[0015] Ag + 50-100%;

[0016] Ag 0 0–49%.

[0017] Secondly, embodiments of the present invention provide a method for preparing a silver-europium co-activated spectral conversion differential phase glass, comprising the following steps:

[0018] (1) Calculate the proportions by mass percentage, weigh out the powdered raw materials including H3BO3, Al2O3, AgNO3, BaCO3, BaF2 and EuF3, mix them, grind them thoroughly and evenly, and melt them fully in an air atmosphere;

[0019] (2) After pouring the molten liquid obtained in step (1) into a mold to form a glass block, a glass block is obtained.

[0020] (3) Take the glass block obtained in step (2) out of the mold, heat it in air atmosphere, and after surface grinding and polishing, make it into sheet glass.

[0021] Further, step (1) includes: melting the powdered raw material in an air atmosphere at 1400-1425°C for 45-55 minutes.

[0022] Further, step (2) includes setting the temperature of the mold to 250°C.

[0023] Further, step (3) includes: taking the glass block obtained in step (2) out of the mold, annealing it at 300°C in air for 18 to 24 hours, and then grinding it with a surface and polishing it with alcohol to make a sheet of glass.

[0024] The beneficial effects of this invention are as follows:

[0025] This invention suppresses the excessive reduction of silver by introducing negatively charged tetrahedra (B, Al, Ba), reducing the likelihood of silver nanoparticle formation and achieving optical stability of silver. The prepared UV-resistant glass layer can efficiently absorb ultraviolet photons, using Ag to absorb photons in the UVB and UVC regions and utilizing Eu... 2+ Absorbing photons from ultraviolet (UVA) significantly improves the stability of perovskite solar cells under ultraviolet irradiation. Simultaneously, through Eu... 3+The red-orange light emission can further improve the device performance of perovskite solar cells. Enriching the two components in different regions—specifically, Ag doping in the boron-rich phase and Eu doping in the fluorine-rich phase—prevents the formation of redox ion pairs caused by Ag / Eu co-doping. Since phase-separated glasses are prone to devitrification, introducing alkaline earth metal ions into the glass can, on the one hand, form a large number of negatively charged polyhedra to suppress excessive silver reduction, and on the other hand, achieve a uniform glass structure, resulting in extremely small phase separations.

[0026] Eu in glass 3+ It would originally spontaneously revert to Eu 2+ However, when it is introduced into silver-containing glass, due to Ag... + Eu has stronger oxidizing properties. 2+ It is oxidized, thus producing Eu 3+ and Ag 0 This process not only promotes the growth of Ag in the glass + The reduction also causes [Ag] in the glass to be reduced. m ] n+ Increased concentration and increased luminescence intensity. Conversely, Ag + The concentration of Eu decreased. 3+ The luminescence occurs via an ff transition, characterized by excitation with violet-blue light and emission with red-orange light. The glass contains both silver and europium luminescent centers, utilizing [Ag]... m ] n+ and Ag + All will be with Eu 3+ The mechanism of energy transfer can further broaden Eu 3+ The excitation bandwidth. The appropriate amount of BaO oxide containing the cation Ba... 2+ With Ag + Competition for neighboring polyhedral sites with non-equilibrium charges can also promote Ag. + Restored to Ag 0 And thus with Ag + Aggregates to form silver quantum clusters [Ag m ] n+ ; with Eu 3+ In comparison, Ba 2+ The electric field strength is relatively small, therefore its ability to release free oxygen is stronger, and its accumulation effect is relatively weak, making Eu... 3+ thanba 2+ It is even more difficult to move from the network. With Eu 3+ Gradually replacing Ba 2+ The accumulation effect is more significant, and the Eu field strength is high. 3+ This makes network connections more robust. Therefore, Eu 3+ thanba 2+This is more conducive to the stability of the glass network. With the addition of various negatively charged alkaline earth metal oxygen polyhedra and the control of Eu concentration, the reduction of silver can be effectively suppressed, thereby effectively suppressing the precipitation of uncharged silver particles in the glass. Combined with the further introduction of BaF2, the transmittance of the glass in the visible region is guaranteed to reach more than 90%.

[0027] Compared with existing technologies, the glass described in this invention exhibits high radiation resistance in the UVA, UVB, and UVC regions, effectively preventing ultraviolet photons from degrading the materials in perovskite solar cells. Furthermore, by utilizing spectral conversion characteristics, ultraviolet photons are modulated into visible light, increasing the utilization rate of visible photons in perovskite solar cells, and further enhancing photoelectric conversion efficiency by utilizing near-infrared light. In addition, all components of the glass of this invention are inorganic, possessing excellent mechanical and physicochemical stability. Attached Figure Description

[0028] To more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0029] Figure 1 The XRD pattern is shown in Example 1 of this invention.

[0030] Figure 2 This is the DTA curve of the silver europium co-activated spectral conversion differential phase glass prepared in Example 1 of this invention;

[0031] Figure 3 This is the XPS Ag 3d peak pattern of the silver-europium co-activated spectral conversion differential phase glass prepared in Example 1 of this invention;

[0032] Figure 4 The normalized fluorescence spectra of excitation and emission intensities of the silver europium co-activated spectral conversion differential phase glass prepared in Example 1 of this invention are shown; the left side of the figure is the excitation spectrum, with the emission wavelength monitored at 616 nm; the right side is the emission spectrum, with the excitation wavelength monitored at 394 nm. Detailed Implementation

[0033] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0034] It should be noted that, unless otherwise specified, the features in the following embodiments and implementation methods can be combined with each other.

[0035] This invention provides a silver-europium co-activated spectral conversion differential phase glass, which contains a boron-rich phase and a fluorine-rich phase, and has the following composition by mass percentage:

[0036] Silver-doped boron-rich phase: 60–75%;

[0037] Europium-doped fluorine-rich phase: 25-40%.

[0038] Furthermore, the silver-doped boron-rich phase has the following elemental composition by mass percentage:

[0039]

[0040] Furthermore, in the silver-doped boron-rich phase of the silver-europium co-activated spectral conversion differential phase glass, Ag is in the +1 valence phase. + Ions and Ag with zero oxidation state 0 They exist in atomic form, and the total content of Ag in both forms is as follows:

[0041] Ag + 50-100%;

[0042] Ag 0 0–49%.

[0043] Furthermore, the europium-doped fluorine-rich phase has the following elemental composition by mass percentage:

[0044] F 15~30%;

[0045] Ba 65%–84%;

[0046] Eu 0.5–10%.

[0047] This invention also provides a method for preparing a silver-europium co-activated spectral conversion differential phase glass, comprising the following steps:

[0048] (1) Calculate the proportions by mass percentage, weigh out the powdered raw materials including H3BO3, Al2O3, AgNO3, BaCO3, BaF2 and EuF3, mix them, grind them thoroughly and evenly, and melt them fully in an air atmosphere;

[0049] Specifically, the melting process in step (1) includes melting the powdered raw material in an air atmosphere at 1400-1425°C for 45-55 minutes.

[0050] (2) After pouring the molten liquid obtained in step (1) into a mold to form a glass block, a glass block is obtained.

[0051] Specifically, in this example, the temperature of the mold is set to 250°C.

[0052] (3) Take the glass block obtained in step (2) out of the mold, heat it in air atmosphere, and after surface grinding and polishing, make it into sheet glass.

[0053] Specifically, the annealing process in step (3) includes: taking the glass block obtained in step (2) out of the mold, annealing it at 300°C in air for 18 to 24 hours, and then grinding it with a surface and polishing it with alcohol to make a sheet of glass.

[0054] It should be noted that in the silver-europium co-activated spectral conversion differential phase glass provided by this invention, the Ag content can be appropriately reduced by introducing small amounts of europium and barium. + The solubility of Ag promotes + Reduced to Ag 0 Furthermore Ag + Ag 0 Ag aggregates to form low-polymerization [Ag] m ] n+ Simultaneously, negatively charged boron-oxygen tetrahedra [BO4] are formed. - Aluminum-oxygen tetrahedron [AlO4] - Barium-oxygen tetrahedron [BaO4] 2- And non-bridging oxygen can suppress the multi-level reduction of silver and effectively inhibit the formation of Ag NPs. Ag-attributed compounds can be observed in the excitation spectrum. + The excitation band (~260nm) still exists in the glass. + And Eu 2+ +Ag + →Eu 3+ +Ag 0 Ag 0 and Ag + Aggregation generates [Ag] m ] n+ Ag + The stronger oxidizing power indicates that the reaction between Ag and Eu can proceed completely, and all Eu in the glass is Eu. 3+ It exists in form. Therefore, it introduces a form greater than Ag. + Eu with low oxidizing power 2+ It will promote the growth of Ag in glass. + Reduction, causing [Ag] in the glass to be reduced. m ] n+ As concentration increases, [Ag] m ] n+ The luminescence intensity increased, while Ag + The concentration decreased. Simultaneously, with the increase of Eu introduction into the glass, Ag concentration decreased.+ / [Ag m ] n+ The decrease in the excitation band intensity ratio indicates that Ag in the glass... + and [Ag] m ] n+ With increased concentration, some Ag + Reduced to Ag 0 Ag 0 and Ag + Aggregates to generate more [Ag] m ] n+ The emission spectrum contains a more pronounced Eu wave in the 570nm–700nm band. 3+: : 5 D0→ 7 F J Linear spectra induced by (J=0~4)ff transitions. Therefore, the main luminescent centers in appropriately europium-doped glass systems are [Ag]... m ] n+ and Eu 3+ excluding Eu 2+ Furthermore, the luminescence intensity is higher than that of the undoped europium glass system, while excessive europium doping will cause the glass to devitrify. Therefore, it is necessary to strictly control the relative ratio of Ag and Eu so that Ag... + With Ag 0 They coexist in glass, and Ag + The relative proportion is not less than 5%. Furthermore, since Ag / Eu co-doping creates redox ion pairs (one reducing and one oxidizing), it is necessary to enrich the two in different regions: Ag in the boron-rich phase and Eu in the fluorine-rich phase. Because phase-separated glasses are prone to devitrification, alkaline earth metal ions are further introduced to address this issue, achieving a uniform glass structure and obtaining extremely small phase separations. Using the above strategy, this invention can prepare inorganic transparent glasses that possess both a large absorption coefficient in the ultraviolet band and high luminous efficiency in the visible band.

[0055] In the inorganic glass network prepared by this invention, because the size of the silver quantum clusters is at the molecular scale, i.e. sub-nanometer level, the concentration of europium doping is low and the spatial distribution is uniform, the average transmittance of the glass in the visible light range is above 91%, which will not affect the photovoltaic performance of perovskite solar cells in the visible band.

[0056] In this invention, an inorganic glass network is employed, utilizing a typical alkaline earth boroaluminosilicate system. Further adjustments to the europium doping concentration effectively stabilize [Ag]... m ] n+ The fluorescence properties and size uniformity of the sample effectively suppress the formation of AgNPs and introduce new luminescent centers, such as Eu. 3+ It can also improve the physicochemical stability and heat resistance of the glass matrix.

[0057] Therefore, the glass described in this invention has high UV radiation resistance and stability, can effectively absorb UV photons and efficiently convert them into broadband fluorescence in the visible blue-green and red-orange bands, and also has high visible transmittance as well as excellent water resistance and heat resistance. It can be made into sheet glass for use as a down-conversion spectral conversion material to modulate the solar spectrum, which can effectively solve the problems of poor UV radiation resistance and low UV utilization in perovskite solar cells, thereby improving the photoelectric conversion efficiency of perovskite solar cells.

[0058] Example 1

[0059] Example 1 of this invention provides a silver-europium co-activated spectral conversion differential phase glass, the preparation process of which is as follows:

[0060] Calculate the mass percentages of H3BO3, Al2O3, AgNO3, BaCO3, BaF2, and EuF3 according to the composition B:Al:Ag:Ba:Eu:O:F = 8.7:7.1:21.3:28.8:0.2:27.6:6.3, and weigh each raw material according to the proportions. Mix the raw material powders of H3BO3, Al2O3, AgNO3, BaCO3, BaF2, and EuF3 evenly in an agate mortar, then transfer the mixed powder to a corundum crucible and melt it in air at 1400℃ for 45 minutes. Pour the molten liquid into a mold at 250℃ for rapid molding. Remove the molded glass block from the mold and anneal it in air at 300℃ for 24 hours. After surface grinding and polishing, it is made into sheet-like transparent glass.

[0061] The obtained sheet-like transparent glass was tested. XRD analysis showed that the glass sample was an amorphous phase, such as... Figure 1 As shown. DTA analysis indicates that the glass transition temperature of this glass is 512.89℃, and the crystallization peak temperature is 671.86℃. Figure 2 As shown. X-ray photoelectron spectroscopy analysis indicates that 55.28% of the Ag element is in the +1 oxidation state. + The ions were present, with 44.72% being Ag with a oxidation state of 0. 0 Atoms exist, such as Figure 3 As shown. Fluorescence spectroscopy indicates that the inorganic transparent glass contains silver quantum clusters and Eu in the ultraviolet band (250–360 nm). 3+ A broad excitation band was observed, with the monitored emission wavelength at 616 nm; a broad emission band of silver quantum clusters was observed in the visible band (380–550 nm), and Eu was observed in the visible band (550 nm–800 nm). 3+ The red-orange light emission peak was monitored at an excitation wavelength of 394 nm. Figure 4As shown. EDX energy dispersive spectroscopy analysis revealed its actual elemental composition to be: B:Al:Ag:Ba:Eu:O:F = 7.7:7.3:21.8:29.5:0.2:27.8:5.7, indicating a certain amount of boron and fluorine volatilization during the preparation process. STEM-EDX surface scanning analysis of silver showed a large number of uniformly sized nanoscale silver quantum clusters distributed within the glass of this embodiment. Transmission spectroscopy indicated that the average transmittance of the glass in the visible band was above 91%. Powder titration analysis determined the hydrolysis grade of the glass in this embodiment to be 3, demonstrating good water resistance and chemical stability.

[0062] Therefore, the silver europium co-activated spectral conversion differential phase glass of the present invention has excellent characteristics such as large absorption coefficient in the ultraviolet band, high broadband fluorescence efficiency in the red and orange bands, high visible transmittance, and stable physicochemical properties. It can be made into sheet glass and used as an anti-ultraviolet radiation layer and spectral conversion material for perovskite solar cells. It is used to modulate ultraviolet light in the solar spectrum into visible light, which can effectively solve the problems of poor ultraviolet radiation resistance and low utilization rate in the ultraviolet region of perovskite solar cells, thereby improving the photoelectric conversion efficiency of perovskite solar cells.

[0063] Example 2

[0064] Example 2 of this invention provides a silver-europium co-activated spectral conversion differential phase glass, the preparation process of which is as follows:

[0065] Calculate the mass percentages of H3BO3, Al2O3, AgNO3, BaCO3, BaF2, and EuF3 according to the composition B:Al:Ag:Ba:Eu:O:F = 8.7:7.1:21.4:28.4:0.5:27.6:6.3, and weigh each raw material according to the proportions. Mix the raw material powders of H3BO3, Al2O3, AgNO3, BaCO3, BaF2, and EuF3 evenly in an agate mortar, then transfer the mixed powder to a corundum crucible and melt it in air at 1400℃ for 45 minutes. Pour the molten liquid into a mold at 250℃ for rapid molding. Remove the molded glass block from the mold and anneal it in air at 300℃ for 24 hours. After surface grinding and polishing, it is made into sheet-like transparent glass.

[0066] The obtained sheet-like transparent glass was tested. XRD analysis showed that the glass sample was amorphous. DTA analysis showed that the glass transition temperature was 508.05℃ and the crystallization peak temperature was 659.43℃. X-ray photoelectron spectroscopy analysis showed that 57.63% of the Ag element was in the +1 valence state. + The ions were present, with 42.37% being Ag in 0 valence. 0Atoms are present. Fluorescence spectroscopy indicates that the inorganic transparent glass contains silver quantum clusters and Eu in the ultraviolet range (250–360 nm). 3+ A broad excitation band was observed, with the monitored emission wavelength at 446 nm; a broad emission band of silver quantum clusters was observed in the visible band (380–550 nm), and Eu was observed in the visible band (550 nm–800 nm). 3+ The glass exhibits a red-orange emission peak, with a monitored excitation wavelength of 382 nm. EDX energy dispersive spectroscopy analysis revealed its actual elemental composition to be: B:Al:Ag:Ba:Eu:O:F = 7.2:7.3:22.1:29.3:0.5:28.2:5.4, indicating a certain amount of boron and fluorine volatilization during the preparation process. STEM-EDX surface scanning analysis of silver showed a large number of uniformly sized nanoscale silver quantum clusters distributed within the glass of this embodiment. Transmission spectroscopy indicated an average visible light transmittance of over 91%. Powder titration determined the glass of this embodiment to have a hydrolysis grade of 3, demonstrating good water resistance and chemical stability.

[0067] Therefore, the silver europium co-activated spectral conversion differential phase glass of the present invention has excellent characteristics such as large absorption coefficient in the ultraviolet band, high broadband fluorescence efficiency in the red and orange bands, high visible transmittance, and stable physicochemical properties. It can be made into sheet glass and used as an anti-ultraviolet radiation layer and spectral conversion material for perovskite solar cells. It is used to modulate ultraviolet light in the solar spectrum into visible light, which can effectively solve the problems of poor ultraviolet radiation resistance and low utilization rate in the ultraviolet region of perovskite solar cells, thereby improving the photoelectric conversion efficiency of perovskite solar cells.

[0068] Example 3

[0069] Example 3 of this invention provides a silver-europium co-activated spectral conversion differential phase glass, the preparation process of which is as follows:

[0070] Calculate the mass percentages of H3BO3, Al2O3, AgNO3, BaCO3, BaF2, and EuF3 according to the composition B:Al:Ag:Ba:Eu:O:F = 8.8:7.2:21.5:27.3:1.0:27.8:6.4, and weigh each raw material according to the proportions. Mix the raw material powders of H3BO3, Al2O3, AgNO3, BaCO3, BaF2, and EuF3 evenly in an agate mortar, transfer the mixed powder to a corundum crucible, and melt it in air at 1400℃ for 45 minutes. Pour the molten liquid into a mold at 250℃ for rapid molding. Remove the molded glass block from the mold and anneal it in air at 300℃ for 24 hours. After surface grinding and polishing, it is made into sheet-like transparent glass.

[0071] The obtained sheet-like transparent glass was tested. XRD analysis showed that the glass sample was amorphous. DTA analysis showed that the glass transition temperature was 501.64℃ and the crystallization peak temperature was 649.91℃. X-ray photoelectron spectroscopy analysis showed that 59.11% of the Ag element was in the +1 valence state. + The ions are present, 40.89% as Ag with a valence of 0. 0 Atoms are present. Fluorescence spectroscopy indicates that the inorganic transparent glass contains silver quantum clusters and Eu in the ultraviolet range (250–360 nm). 3+ A broad excitation band was observed, with the monitored emission wavelength at 444 nm; a broad emission band of silver quantum clusters was observed in the visible band (380–550 nm), and Eu was observed in the visible band (550 nm–800 nm). 3+ The glass exhibits a red-orange emission peak, with a monitored excitation wavelength of 380 nm. EDX energy dispersive spectroscopy analysis revealed its actual elemental composition to be: B:Al:Ag:Ba:Eu:O:F = 7.4:7.3:21.9:27.8:1.0:28.5:6.1, indicating a certain amount of boron and fluorine volatilization during the preparation process. STEM-EDX surface scanning analysis of silver showed a large number of uniformly sized nanoscale silver quantum clusters distributed within the glass of this embodiment. Transmission spectroscopy indicated an average visible light transmittance of over 92%. Powder titration determined the glass of this embodiment to have a hydrolysis grade of 3, demonstrating good water resistance and chemical stability.

[0072] Therefore, the silver europium co-activated spectral conversion differential phase glass of the present invention has excellent characteristics such as large absorption coefficient in the ultraviolet band, high broadband fluorescence efficiency in the red and orange bands, high visible transmittance, and stable physicochemical properties. It can be made into sheet glass and used as an anti-ultraviolet radiation layer and spectral conversion material for perovskite solar cells. It is used to modulate ultraviolet light in the solar spectrum into visible light, which can effectively solve the problems of poor ultraviolet radiation resistance and low utilization rate in the ultraviolet region of perovskite solar cells, thereby improving the photoelectric conversion efficiency of perovskite solar cells.

[0073] Example 4

[0074] Example 4 of this invention provides a silver-europium co-activated spectral conversion differential phase glass, the preparation process of which is as follows:

[0075] Calculate the mass percentages of H3BO3, Al2O3, AgNO3, BaCO3, BaF2, and EuF3 according to the composition B:Al:Ag:Ba:Eu:O:F = 8.9:7.3:21.9:25.2:2.1:28.0:6.6, and weigh each raw material according to the proportions. Mix the raw material powders of H3BO3, Al2O3, AgNO3, BaCO3, BaF2, and EuF3 evenly in an agate mortar, transfer the mixed powder to a corundum crucible, and melt it in air at 1400℃ for 45 minutes. Pour the molten liquid into a mold at 250℃ for rapid molding. Remove the molded glass block from the mold and anneal it in air at 300℃ for 24 hours. After surface grinding and polishing, it is made into sheet-like transparent glass.

[0076] The obtained sheet-like transparent glass was tested. XRD analysis showed that the glass sample was amorphous. DTA analysis showed that the glass transition temperature was 499.92℃ and the crystallization peak temperature was 647.73℃. X-ray photoelectron spectroscopy analysis showed that 62.62% of the Ag element was in the +1 valence state. + The ions were present, 37.38% as Ag with a valence of 0. 0 Atoms are present. Fluorescence spectroscopy indicates that the inorganic transparent glass contains silver quantum clusters and Eu in the ultraviolet range (250–360 nm). 3+ A broad excitation band was observed, with the monitored emission wavelength at 443 nm; a broad emission band of silver quantum clusters was observed in the visible band (380–550 nm), and Eu was observed in the visible band (550 nm–800 nm). 3+ The glass exhibits a red-orange emission peak, with a monitored excitation wavelength of 372 nm. EDX energy dispersive spectroscopy analysis revealed its actual elemental composition to be: B:Al:Ag:Ba:Eu:O:F = 7.5:7.6:22.8:26.3:2.2:27.3:6.3, indicating a certain amount of boron and fluorine volatilization during the preparation process. STEM-EDX surface scanning analysis of silver showed a large number of uniformly sized nanoscale silver quantum clusters distributed within the glass of this embodiment. Transmission spectroscopy indicated an average visible light transmittance of over 92%. Powder titration determined the glass of this embodiment to have a hydrolysis grade of 3, demonstrating good water resistance and chemical stability.

[0077] Therefore, the silver europium co-activated spectral conversion differential phase glass of the present invention has excellent characteristics such as large absorption coefficient in the ultraviolet band, high broadband fluorescence efficiency in the red and orange bands, high visible transmittance, and stable physicochemical properties. It can be made into sheet glass and used as an anti-ultraviolet radiation layer and spectral conversion material for perovskite solar cells. It is used to modulate ultraviolet light in the solar spectrum into visible light, which can effectively solve the problems of poor ultraviolet radiation resistance and low utilization rate in the ultraviolet region of perovskite solar cells, thereby improving the photoelectric conversion efficiency of perovskite solar cells.

[0078] The above embodiments are used to explain and illustrate the present invention, but not to limit the present invention. Any modifications and changes made to the present invention within the spirit and scope of the claims shall fall within the protection scope of the present invention.

Claims

1. A silver-europium co-activated spectral conversion differential phase glass, characterized in that, The silver-europium co-activated spectral conversion differential phase glass contains a silver-doped boron-rich phase and a europium-doped fluorine-rich phase. XRD analysis shows that the silver-europium co-activated spectral conversion differential phase glass is an amorphous phase, and all Eu in the glass exists in the form of Eu³⁺. By mass percentage, the silver-europium co-activated spectral conversion differential phase glass has the following composition: Silver-doped boron-rich phase: 60–75%; Europium-doped fluorine-rich phase: 25-40%; The silver-doped boron-rich phase has the following elemental composition by mass percentage: O 35~45%; B 8~20%; Al 5~16%; Ba 4-14%; Ag 25-35%; The europium-doped fluorine-rich phase has the following elemental composition by mass percentage: F 15~30%; Ba 65-84%; Eu 0.5–10%; In the silver-doped boron-rich phase, Ag exists as Ag⁺ ions with a +1 valence and Ag⁺ ions with a valence of 0 valence. 0 They exist in atomic form, and the total content of Ag in both forms is as follows: Ag⁺ 50~100%; At 0 0~49%.

2. A method for preparing the silver-europium co-activated spectral conversion differential phase glass according to claim 1, characterized in that, Includes the following steps: (1) Calculate the proportions by mass percentage, weigh out the powdered raw materials of H3BO3, Al2O3, AgNO3, BaCO3, BaF2 and EuF3, mix them, grind them evenly, and melt them fully in air at 1400-1425℃ for 45-55 minutes; (2) Pour the molten liquid obtained in step (1) into a mold to form a glass block; (3) Take the glass block obtained in step (2) out of the mold, heat it in air atmosphere, and after surface grinding and polishing, make it into sheet glass.

3. The method for preparing silver-europium co-activated spectral conversion differential phase glass according to claim 2, characterized in that, In step (2), the temperature of the mold is set to 250°C.

4. The method for preparing silver-europium co-activated spectral conversion differential phase glass according to claim 2, characterized in that, Step (3) includes: taking the glass block obtained in step (2) out of the mold, annealing it at 300°C in air for 18 to 24 hours, and then grinding it with a surface and polishing it with alcohol to make a sheet of glass.

Citation Information

Patent Citations

  • Multicolor silver quantum cluster doped multiphase fluorescent glass and preparation method thereof

    CN111018348A