A heavy oil hydroprocessing catalyst, its preparation method and application

By pretreating the regenerated hydrotreating catalyst and introducing pseudoboehmite molding treatment, the pore structure of the heavy oil hydrotreating catalyst was improved, the problem of reduced activity caused by carbon deposits was solved, and efficient removal of asphaltenes and metal impurities was achieved, thereby improving the catalyst utilization rate and environmental friendliness.

CN118207016BActive Publication Date: 2026-11-20PETROCHINA CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211622238.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-16
Publication Date
2026-11-20
Estimated Expiration
2042-12-16

AI Technical Summary

Technical Problem

Existing heavy oil hydrotreating catalysts are difficult to regenerate effectively after carbon buildup leads to reduced activity. Furthermore, high-temperature treatment can cause active metal aggregation and pore structure damage, resulting in poor deasphalting and demetallization effects.

Method used

Pretreatment of the regenerated hydrotreating catalyst involves introducing pseudoboehmite and shaping it to improve the pore structure and prevent the aggregation of active metals, thereby preparing a high-efficiency heavy oil hydrotreating catalyst.

Benefits of technology

This method improves the catalytic activity of the catalyst, effectively removes asphaltenes and metallic impurities from the feedstock, solves the catalyst contamination problem, and is simple, easy to implement, and has low energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004002876630000091
    Figure BDA0004002876630000091
  • Figure BDA0004002876630000101
    Figure BDA0004002876630000101
  • Figure BDA0004002876630000102
    Figure BDA0004002876630000102
Patent Text Reader

Abstract

The application provides a heavy oil hydroprocessing catalyst, a preparation method and application thereof, and the preparation method comprises the following steps: pretreating a to-be-regenerated hydrogenation catalyst to obtain a pretreated hydrogenation catalyst; the pretreatment at least comprises a deoiling treatment; mixing the pretreated hydrogenation catalyst, pseudo-boehmite, a binder and water to form a mixture, and mixing and kneading the mixture to form a formed body; and drying and calcining the formed body to obtain the heavy oil hydroprocessing catalyst. The heavy oil hydroprocessing catalyst with excellent deasphaltene and demetallization rates can be prepared while the to-be-regenerated hydrogenation catalyst is fully utilized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of catalysts, specifically relating to a heavy oil hydrotreating catalyst, its preparation method, and its application. Background Technology

[0002] During the hydrogenation reaction, the activity of the hydrogenation catalyst gradually decreases with prolonged operation, rendering it unusable. Since these unusable spent catalysts still contain active metals such as vanadium, molybdenum, cobalt, and nickel, directly discarding them not only wastes resources and increases production costs but also pollutes the environment. Regenerating and reusing spent catalysts is a breakthrough in improving catalyst utilization, reducing production costs, and solving pollution problems.

[0003] The main cause of catalyst deactivation is the formation of carbon deposits. Currently, catalyst activity can be restored by carbon removal, for example, through high-temperature treatment. However, high-temperature treatment can lead to the aggregation of active metals, resulting in significant activity loss. Furthermore, it can damage the original pore structure of the catalyst, hindering the diffusion of feedstock oil and ultimately leading to poor deasphalting and demetallization of the regenerated catalyst. Therefore, how to fully utilize spent catalysts to obtain heavy oil hydrotreating catalysts with high deasphalting and demetallization rates has been a long-standing research topic in this field. Summary of the Invention

[0004] This invention provides a method for preparing a heavy oil hydrotreating catalyst. First, the hydrotreating catalyst to be regenerated is pretreated. Then, pseudoboehmite is introduced and shaped to improve the pore structure of the hydrotreating catalyst, preventing the aggregation of active metals and thus enhancing its catalytic activity, particularly the deasphalting and demetallization rates. Simultaneously, the active metals in the hydrotreating catalyst to be regenerated are fully utilized, solving the contamination problem of the catalyst and enabling the preparation of a heavy oil hydrotreating catalyst with excellent deasphalting and demetallization performance.

[0005] This invention also provides a heavy oil hydrotreating catalyst, which has high catalytic activity. This hydrotreating catalyst is particularly effective in removing impurities such as asphaltenes and metals from feedstock oil, and is especially suitable for the hydrotreating and conversion of inferior heavy oil with high metal and asphaltenes content.

[0006] This invention also provides a method for hydrotreating heavy oil, which has advantages such as good hydrotreating effect.

[0007] In one aspect, the present invention provides a method for preparing a heavy oil hydrotreating catalyst, comprising the following steps:

[0008] The hydrogenation catalyst to be regenerated is pretreated to obtain a pretreated hydrogenation catalyst; the pretreatment includes at least an oil removal process.

[0009] The pretreated hydrogenation catalyst, pseudoboehmite, binder and water are mixed to form a mixture, which is then kneaded and molded to obtain a molded body.

[0010] The molded body is dried and calcined to obtain a heavy oil hydrotreating catalyst.

[0011] According to one embodiment of the present invention, the mass ratio of pseudoboehmite to the pretreatment hydrogenation catalyst is (0.5-1.5):1.

[0012] According to one embodiment of the present invention, the hydrogenation catalyst to be regenerated is 20-80% of the mass content of the hydrogenation treatment catalyst.

[0013] According to one embodiment of the present invention, the preprocessing includes:

[0014] The hydrogenation catalyst to be regenerated is sequentially screened and deoiled, and then the material obtained after deoiling is crushed.

[0015] According to one embodiment of the present invention, the deoiling process involves sequentially eluting and drying the sieved catalyst with an organic solvent, wherein the organic solvent is selected from at least one of ethanol, petroleum ether, and gasoline, the elution temperature is 20–80°C, and the drying temperature is 80–180°C.

[0016] Alternatively, the deoiling process may involve dry distillation or stripping of the sieved catalyst using an inert gas, with the dry distillation or stripping temperature being 200–450°C.

[0017] According to one embodiment of the present invention, the mixture further includes an auxiliary agent, said auxiliary agent including at least one selected from guar gum powder, methylcellulose, starch, polyvinyl alcohol, and polyacrylamide.

[0018] According to one embodiment of the present invention, the drying temperature is 80-150°C and the drying time is 1-8 hours.

[0019] According to one embodiment of the present invention, the calcination is carried out in an oxygen-containing atmosphere, the calcination temperature is 400-1300°C, and the calcination time is 0.5-6 hours.

[0020] According to one embodiment of the present invention, the oxygen-containing atmosphere is oxygen or a mixture of oxygen and a carrier gas, wherein the volume content of oxygen in the mixture is 2-15%.

[0021] In a second aspect, the present invention provides a heavy oil hydrotreating catalyst, which is obtained by the preparation method described above.

[0022] According to one embodiment of the present invention, the heavy oil hydrotreating catalyst has the following properties: a specific surface area of ​​10 to 400 m². 2 / g, with a total pore volume of 0.2-3mL / g, and the pore volume of macropores larger than 100nm accounts for more than 10% of the total pore volume.

[0023] In a third aspect, the present invention provides a method for hydrotreating heavy oil, using the above-described heavy oil hydrotreating catalyst.

[0024] The implementation of this invention has at least the following beneficial effects:

[0025] The method for preparing a heavy oil hydrotreating catalyst provided by this invention first pretreats the hydrogenation catalyst to be regenerated, making it part of the heavy oil hydrotreating catalyst, thereby improving the utilization rate of the support and active metal in the hydrogenation catalyst to be regenerated; then, pseudoboehmite is introduced into the pretreated hydrogenation catalyst and shaped, and through drying and calcination, the proportion of macropores in the support is increased, the pore structure of the catalyst is improved, and the aggregation of active metal is avoided, thus obtaining a heavy oil hydrotreating catalyst with high catalytic activity, which can effectively remove asphaltenes, metals and other impurities from the feedstock oil.

[0026] The method for preparing heavy oil hydrotreating catalyst provided by this invention is particularly suitable for recycling heavy and sludge oil hydrotreating catalysts whose activity has been reduced due to carbon deposits. In addition, it has the advantages of simple method, easy implementation and low energy consumption. Detailed Implementation

[0027] The specific embodiments listed below are merely descriptions of the principles and features of the present invention. The examples given are only for explaining the present invention and are not intended to limit the scope of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0028] This invention provides a method for preparing a heavy oil hydrotreating catalyst, comprising the following steps: pretreating the hydrogenation catalyst to be regenerated to obtain a pretreated hydrogenation catalyst, wherein the pretreatment includes at least an oil removal process; mixing the pretreated hydrogenation catalyst, boehmite, binder, and water to form a mixture, and kneading and molding the mixture to obtain a molded body; drying and calcining the molded body to obtain the heavy oil hydrotreating catalyst.

[0029] In this invention, the hydrogenation catalyst to be regenerated refers to a hydrogenation catalyst whose activity decreases during the hydrogenation process due to carbon deposition. The preparation method of this invention is particularly suitable for recycling hydrogenation catalysts with a carbon deposition content greater than 10%.

[0030] This invention does not limit the specific type of hydrogenation catalyst to be regenerated. Depending on the hydrogenation feedstock, the hydrogenation catalyst to be regenerated includes distillate oil hydrogenation catalysts and heavy / residue oil hydrogenation catalysts.

[0031] The present invention does not limit the process used for the regenerated hydrogenation catalyst. For example, it can be applied to processes such as hydrodesulfurization, hydrodenitrification, hydrodemetallization, and hydrodeasphalting. The regenerated hydrogenation catalyst of the present invention is particularly suitable for hydrodemetallization and hydrodeasphalting.

[0032] In this invention, the hydrogenation catalyst to be regenerated comprises at least an active metal component and a support. The active metal content on the hydrogenation catalyst to be regenerated is generally 1–20 wt% of the total weight of the catalyst, and the mass of the active metal is based on metal oxides. The active metal component includes, but is not limited to, at least one metal from Group VIB and Group VIII of the periodic table, such as vanadium, molybdenum, cobalt, nickel, and iron. The support includes, but is not limited to, at least one from alumina, silica, titanium dioxide, silicon carbide, boron oxide, zirconium oxide, and molecular sieves.

[0033] In this invention, the boehmite can be a boehmite containing only alumina, or a boehmite containing silicon dioxide, titanium dioxide, zirconium oxide, etc. It should be noted that the support material in the hydrogenation catalyst to be regenerated can be the same as or different from the boehmite material selected in this invention, but preferably the same.

[0034] This invention does not limit the pretreatment process, as long as it can remove impurities from the surface of the hydrogenation catalyst to be regenerated. Since the surface of the hydrogenation catalyst to be regenerated contains impurities such as feedstock oil, targeted degreasing treatment can effectively remove these surface impurities. In this invention, kneading is used to achieve uniform mixing of the materials, resulting in a homogeneous and plastic mixture. Through molding, the mixture is formed into a molded body with a specific shape and size.

[0035] The shape and size of the molded body mainly depend on the molding method. Those skilled in the art can select a specific molding method according to actual needs. Molding methods include, but are not limited to, drop ball molding, rolling ball granulation, extrusion molding, and sheet molding. Correspondingly, the shape of the molded body can be spherical, strip-shaped, sheet-shaped, etc. When the shape of the molded body is strip-shaped, it specifically includes cylindrical, clover-shaped, and four-leaf clover-shaped forms.

[0036] According to the technical solution of the present invention, the catalyst to be regenerated is first pretreated, and then pseudoboehmite is introduced into the pretreated catalyst and shaped to increase the proportion of macropores in the support, improve the pore structure of the catalyst, avoid the aggregation of active metals, and thus enhance the catalytic activity of the heavy oil hydrotreating catalyst. Using this heavy oil hydrotreating catalyst to hydrotreat feedstock oil facilitates the diffusion of the feedstock oil and enables the effective removal of impurities such as asphaltenes and metals from the feedstock oil. Simultaneously, it fully utilizes the active metal components in the catalyst to be regenerated, solving the contamination problem of the catalyst to be regenerated.

[0037] In one embodiment of the present invention, the pretreatment includes: sequentially screening and deoiling the hydrogenation catalyst to be regenerated, and then pulverizing the material obtained after deoiling.

[0038] In the above pretreatment, the sieving process can employ conventional sieving methods in the art to remove excess impurities. The deoiling process can employ conventional deoiling methods in the art, specifically at least one of solvent elution, gas stripping, and dry distillation.

[0039] When the deoiling process is solvent elution, it specifically includes: using organic solvents to sequentially elute and dry the sieved catalyst.

[0040] The organic solvent is selected from at least one of ethanol, petroleum ether, and gasoline. The elution temperature is 20–80°C and the elution time is 1–4 h. The volume ratio of organic solvent to sieved catalyst is (1–4):1. Drying can be carried out under a nitrogen atmosphere by purging and drying at a temperature of 80–180°C, or further 80–150°C.

[0041] When the deoiling process is gas stripping or dry distillation, it specifically includes: using a flowing inert gas to deoil and dry the sieved catalyst.

[0042] The temperature for dry distillation or stripping is 200–450°C, and the inert gas includes at least one of nitrogen, argon, helium, and neon.

[0043] The material obtained after degreasing is then pulverized, specifically by grinding the material obtained after degreasing to 60-400 mesh.

[0044] In one embodiment of the present invention, the pseudoboehmite used is a powder, and the powder has a colloidal solubility of more than 10%.

[0045] In the mixture, the mass ratio of pseudoboehmite to pretreated hydrogenation catalyst is (0.5 to 1.5):1, for example, 0.5:1, 0.8:1, 1:1, 1.2:1, 1.5:1 or any combination thereof.

[0046] During the preparation process, by controlling the amount of pretreatment hydrogenation catalyst added to the mixture, the mass ratio of the hydrogenation catalyst to be regenerated in the heavy oil hydrogenation catalyst can be controlled.

[0047] In this invention, the hydrogenation catalyst to be regenerated comprises 20% to 80% of the heavy oil hydrotreating catalyst by mass, for example, 20%, 30%, 40%, 50%, 60%, 70%, 80%, or any combination thereof. The inventors have discovered that when the hydrogenation catalyst to be regenerated comprises 20% to 80% of the heavy oil hydrotreating catalyst by mass, not only can the support and active metal in the hydrogenation catalyst be utilized to the maximum extent, but the pore structure and strength of the heavy oil hydrotreating catalyst can also be improved, which is beneficial to enhancing the activity of the heavy oil hydrotreating catalyst.

[0048] In this invention, the binder is an inorganic acid and / or an organic acid, specifically including at least one of nitric acid, acetic acid, formic acid, and hydrochloric acid.

[0049] To ensure the smooth progress of the above-mentioned kneading and molding, the mixture also includes additives, including at least one of guar gum powder, methylcellulose, starch, polyvinyl alcohol, and polyacrylamide. The amount of additives added is 0.5% to 20% of the mass of the mixture.

[0050] The pore structure of the carrier can be adjusted by using a pore expander. This invention can introduce a pore expander into the mixture as needed. The pore expander can be at least one of starch, synthetic cellulose, polymeric alcohol, and surfactant. Specifically, synthetic cellulose includes at least one of hydroxymethyl cellulose, methyl cellulose, and ethyl cellulose; polymeric alcohol includes at least one of polyethylene glycol, polypropylene alcohol, and polyvinyl alcohol; and surfactant includes at least one of fatty alcohol polyethylene ether, fatty alcohol amides and their derivatives, propylene alcohol copolymers with a molecular weight of 200-10000, and maleic acid copolymers.

[0051] In this invention, before drying and calcining the molded body, the molded body is further aged at a temperature of 70°C for 2 hours.

[0052] In this invention, the drying temperature for the molded body is 80–150°C, and the drying time is 1–8 hours. Calcination is carried out in an oxygen-containing atmosphere at a temperature of 400–1300°C for 0.5–6 hours. Calcination can be performed in a calcination furnace. This invention does not limit the calcination method; static calcination or dynamic calcination can be used.

[0053] The oxygen-containing atmosphere is oxygen gas, or a mixture of oxygen gas and a carrier gas. The oxygen volume content in the mixture is 2% to 15%, for example, 2%, 4%, 5%, 8%, 10%, 15%, or any combination thereof. The carrier gas is an inert gas, and the inert gas is at least one of helium, neon, and argon.

[0054] This invention also provides a heavy oil hydrotreating catalyst, obtained by the above-described preparation method. The properties of this heavy oil hydrotreating catalyst are as follows: specific surface area of ​​10–400 m² / g. 2 / g, with a total pore volume of 0.2-3mL / g, and the pore volume of macropores larger than 100nm accounts for more than 10% of the total pore volume.

[0055] The present invention also provides a method for hydrotreating heavy oil, wherein the feedstock oil is brought into contact with the above-mentioned heavy oil hydrotreating catalyst to perform hydrotreating.

[0056] This invention provides a heavy oil hydrotreating catalyst and its preparation method. The method involves pretreating the hydrogenation catalyst to be regenerated, introducing boehmite and shaping it, and then drying and calcining it to increase the proportion of macropores (especially those larger than 100 nm) on the support, improving the pore structure of the heavy oil hydrotreating catalyst, and preventing the aggregation of active metals, thereby obtaining a heavy oil hydrotreating catalyst with high catalytic activity. Applying this heavy oil hydrotreating catalyst to the hydrotreating process of feedstock oil can significantly improve the diffusion of feedstock oil and effectively remove asphaltenes, metals, and other impurities. Simultaneously, this preparation method fully utilizes the support portion and its active metal components in the hydrogenation catalyst to be regenerated, solving the pollution problem of the hydrogenation catalyst to be regenerated and achieving efficient resource utilization.

[0057] The methods and effects provided by the embodiments of the present invention will be further explained below through examples and comparative examples, but this does not limit the present invention.

[0058] In the examples and comparative examples, the pseudoboehmite dry adhesive powder was purchased from Shandong Xingdu Petrochemical Technology Co., Ltd.

[0059] Example 1

[0060] The hydrogenation catalyst for removing residual carbon from waste oil after the operation of the industrial plant was used as the hydrogenation catalyst to be regenerated. The catalyst was NiMo / Al2O3 with a carbon deposition of 15.6 wt%.

[0061] The hydrogenation catalyst to be regenerated was eluted with ethanol, continuously washed at 80°C for 2 hours, then dried by nitrogen purging at 100°C for 1 hour, and then pulverized to 150 mesh to obtain pretreated hydrogenation catalyst A; wherein the volume ratio of ethanol to hydrogenation catalyst to be regenerated was 3:1.

[0062] 500g (dry basis) of pseudoboehmite dry adhesive powder (colloidal solubility index of 21%), 300g of pretreated hydrogenation catalyst A, 15g of guar gum powder, and 15g of starch were mixed evenly. 810g of acetic acid solution with a concentration of 2wt% was added to the mixture, and kneaded for 30 minutes. The mixture was then extruded into clover-shaped particles with a particle size of 1.0mm on an extruder and labeled A-1. The mixture was aged at 70℃ for 2 hours, dried at 110℃ for 3 hours, and then placed in a calcination furnace. In an atmosphere with an oxygen volume content of 12%, the temperature was increased to 580℃ at a rate of 100-200℃ / hour and calcined for 3 hours to obtain catalyst A-1C.

[0063] Example 2

[0064] The waste residue oil hydrodesulfurization catalyst after the industrial plant has been in operation was used as the hydrodesulfurization catalyst to be regenerated. The catalyst is CoMo / Al2O3 with a carbon deposition of 12.8 wt%.

[0065] The hydrogenation catalyst to be regenerated was purged at 350°C under a nitrogen atmosphere for 1 hour and then pulverized to 200 mesh to obtain pretreated hydrogenation catalyst B.

[0066] 500g (dry basis) of silicon-containing pseudoboehmite dry adhesive powder (with SiO2 content of 10% and colloidal index of 11%), 500g of pretreated hydrogenation catalyst B, and 15g of guar gum powder were mixed evenly. 950g of 2.0wt% acetic acid solution and 3.0wt% citric acid solution were added and kneaded for 30 minutes. The mixture was then extruded into four-leaf strips with a particle size of Φ1.3mm on an extruder, and designated as A-2. The strips were dried at 120℃ for 3 hours and then placed in a calcining furnace. In an atmosphere with an oxygen volume content of 10%, the temperature was increased to 700℃ at a rate of 100-200℃ / hour and calcined for 3 hours to obtain catalyst A-2C.

[0067] Example 3

[0068] The hydrogenation denitrification catalyst of the waste residue oil after the operation of the industrial plant was used as the hydrogenation catalyst to be regenerated. The catalyst was NiMo / Al2O3 with 21.2 wt% carbon deposit.

[0069] After purging the hydrogenation catalyst to be regenerated under a nitrogen atmosphere at 400°C for 1 hour, it was taken out and crushed to 280 mesh to obtain the pretreated hydrogenation catalyst C.

[0070] 500g (dry basis) of pseudoboehmite dry adhesive powder (with TiO2 content of 10% and colloidal index of 15%) (produced by Shandong Xingdu Petrochemical Technology Co., Ltd.), 650g of pretreated hydrogenation catalyst C, and 15g of guar gum powder were mixed evenly. 1070g of a mixed solution of acetic acid with a concentration of 3.0wt% and citric acid with a concentration of 2.0% was added to the mixture. After kneading, the mixture was extruded into clover strips with a particle size of Φ1.6mm on an extruder, and designated as A-3. The strips were dried at 120℃ for 3 hours and then placed in a calcining furnace. In an atmosphere with an oxygen volume content of 8%, the temperature was increased to 750℃ at a rate of 100-200℃ / hour and calcined for 3 hours to obtain catalyst A-3C.

[0071] Example 4

[0072] The hydrogenation catalyst of the waste deasphalted oil after the operation of the industrial plant was used as the hydrogenation catalyst to be regenerated. The catalyst is NiW / Al2O3 with 23.8wt% carbon deposit.

[0073] After purging the hydrogenation catalyst to be regenerated under a nitrogen atmosphere at 350°C for 1 hour, it was taken out and crushed to 250 mesh to obtain the pretreated hydrogenation catalyst D.

[0074] 500g (dry basis) of pseudoboehmite dry adhesive powder, 800g of pretreated hydrogenation catalyst D, and 15g of guar gum powder were mixed evenly. 1220g of 4.5wt% acetic acid solution was added to the mixture, and kneaded for 30 minutes. The mixture was then extruded into 2.0mm four-leaf clover-shaped particles on a single-screw extruder and labeled A-4. The particles were dried at 120℃ for 3 hours and then placed in a calcining furnace. In an atmosphere with an oxygen volume content of 6%, the temperature was increased to 650℃ at a rate of 100-200℃ / hour and calcined for 3 hours to obtain catalyst A-4C.

[0075] Comparative Example 1

[0076] The hydrogenation catalyst to be regenerated in Example 2 was subjected to carbonization treatment at 550°C in air atmosphere for 2 hours to obtain pretreated hydrogenation catalyst E.

[0077] 500g (dry basis) of silica-containing pseudoboehmite dry adhesive powder (with SiO2 content of 10% and colloidal index of 11%), 500g of the above-mentioned pretreated hydrogenation catalyst E, and 15g of guar gum powder were mixed evenly. 1050g of a mixed solution of acetic acid and citric acid with a concentration of 2.0wt% was added to the mixture. The mixture was then extruded into clover-shaped particles with a particle size of 1.3mm on a single screw extruder. The particles were dried at 120℃ for 3 hours and then placed in a calcining furnace. The temperature was increased to 700℃ at a rate of 100-200℃ / hour and calcined for 3 hours to obtain catalyst D-1.

[0078] Comparative Example 2

[0079] 500g (dry basis) of silica-containing pseudoboehmite dry adhesive powder (with SiO2 content of 10% and colloidal index of 11%) and 15g of guar gum powder were mixed evenly. 475g of a mixed solution of acetic acid with a concentration of 2.0wt% and citric acid with a concentration of 3.0% was added to the mixture and kneaded for 30 minutes. Then, the mixture was extruded into four-leaf clover strips with a particle size of Φ1.3mm on an extruder. The strips were dried at 120℃ for 3 hours and then placed in a calcining furnace. In an air atmosphere, the temperature was increased to 700℃ at a rate of 100-200℃ / hour and calcined for 3 hours to obtain the carrier.

[0080] Weigh 150g of the above-mentioned support (water absorption rate 1.10mL / g), and spray it with 165mL of a solution containing 13g of ammonium heptamolybdate (containing 81wt% MoO3) and 15.7g of nickel nitrate (containing 25.2wt% NiO) according to the saturated absorption solution volume. After homogenization in the spraying equipment for 5 minutes, remove it and dry it at 120℃ for 3 hours, and then calcine it in air at 500℃ for 3 hours to obtain the catalyst, which is denoted as D-2.

[0081] The properties of the hydrogenation catalysts prepared in the above examples and comparative examples are shown in Table 1.

[0082] Table 1 Properties of Hydrotreatment Catalysts

[0083]

[0084]

[0085] In the table, " / " indicates no test results.

[0086] According to Table 1:

[0087] 1. Compared with Comparative Example 1, the heavy oil hydrotreating catalyst in the examples has a larger pore volume, indicating that the preparation method of the examples is beneficial to improving pore volume and pore structure.

[0088] 2. Compared with Comparative Example 2, the heavy oil hydrotreating catalyst in the examples has a larger pore volume, indicating that the pore volume and pore structure of the heavy oil hydrotreating catalyst in the examples are superior to the fresh catalyst prepared by conventional methods.

[0089] 3. When the catalysts to be regenerated used in Comparative Example 1 and Example 2 are exactly the same, the heavy oil hydrotreating catalyst in Example 2 has a larger pore volume and a significantly increased proportion of macropores, indicating that the preparation method of Example 2 is more conducive to improving the pore volume and macropore ratio of the heavy oil hydrotreating catalyst.

[0090] In a 100mL three-stage fixed-bed hydrogenation unit, catalysts A-1C, A-2C, D-1, and D-2 were loaded into the three reactors, and activity and stability tests were conducted on catalysts A-1C, A-2C, D-1, and D-2. For ease of comparison, the first and second reactors were loaded with the same pre-catalysts. The feedstock was a mixed residue oil, the properties of which are shown in Table 2. The evaluation process conditions are shown in Table 3, and the evaluation results are shown in Table 4.

[0091] Table 2 Properties of Crude Oil

[0092]

[0093] Table 3 Hydrogenation Process Conditions

[0094] Pressure, MPa 16.0 <![CDATA[liquid hourly space velocity, h -1 > 0.30 Hydrogen-to-oil ratio (by volume) 550:1 Reaction temperature, °C 380

[0095] Table 4. Evaluation Results of Hydrogenation

[0096]

[0097] In the table, the deasphalting rate, desulfurization rate, and demetallization rate represent the relative deasphalting rate, relative desulfurization rate, and relative demetallization rate. Specifically, the deasphalting rate, desulfurization rate, and demetallization rate of A-1C and catalyst running for 500 hours are compared with a benchmark of 1.00.

[0098] According to Table 4:

[0099] 1. The relative demetallization rate and relative deasphalting rate of catalysts A-1C and A-2C are both higher than those of D-1 and D-2, indicating that the hydrotreating catalysts in the examples exhibit good catalytic activity. The inventors speculate that the high macroporous ratio of the hydrotreating catalysts in the examples is beneficial to the diffusion, conversion, and removal of macromolecules in the feedstock oil;

[0100] 2. As operation continued, the relative demetallization rate and relative deasphalting rate of catalysts A-1C and A-2C decreased by no more than 15%, while the decrease rate of D-1 and D-2 even reached more than 25%. This indicates that the catalysts in the examples exhibited good stability, were able to maintain long-term operation, and had a long service life.

[0101] The preferred embodiments and experimental verifications of the present invention have been described in detail above. It should be understood that those skilled in the art can make numerous modifications and variations based on the concept of the present invention without creative effort. Therefore, all technical solutions that can be obtained by those skilled in the art based on the concept of the present invention through logical analysis, reasoning, or limited experimentation on the basis of existing technology should be within the scope of protection defined by the claims.

Claims

1. A method for preparing a catalyst for heavy oil hydrotreating, characterized in that, Includes the following steps: The hydrogenation catalyst to be regenerated is pretreated to obtain a pretreated hydrogenation catalyst. The carbon content of the hydrogenation catalyst to be regenerated is greater than 10%; the pretreatment includes: sequentially screening and deoiling the hydrogenation catalyst to be regenerated, and then pulverizing the material obtained after deoiling; the deoiling process involves sequentially washing and drying the screened catalyst with an organic solvent, wherein the organic solvent is selected from at least one of ethanol, petroleum ether, and gasoline, the washing temperature is 20~80℃, and the drying temperature is 80~180℃; or, the deoiling process involves dry distillation or stripping the screened catalyst with an inert gas, the dry distillation or stripping temperature is 200~450℃; A mixture is formed by mixing a pretreated hydrogenation catalyst, boehmite, a binder, and water, and then kneading and molding the mixture to obtain a molded body. The binder is an inorganic acid and / or an organic acid; the boehmite is a powder with a colloidal solubility greater than 10%. The molded body is dried and calcined to obtain a heavy oil hydrotreating catalyst; the calcination is carried out in an oxygen-containing atmosphere at a temperature of 400–1300 °C. The heavy oil hydrotreating catalyst has the following properties: specific surface area of ​​10–400 m². 2 / g, with a total pore volume of 0.2-3mL / g, and the pore volume of macropores larger than 100nm accounts for more than 10% of the total pore volume.

2. The preparation method according to claim 1, characterized in that, The mass ratio of the pseudoboehmite to the pretreated hydrogenation catalyst is (0.5~1.5):

1.

3. The preparation method according to claim 1, characterized in that, The hydrogenation catalyst to be regenerated is 20-80% of the mass content of the hydrogenation treatment catalyst.

4. The preparation method according to any one of claims 1-3, characterized in that, The mixture also includes additives, which include at least one of guar gum powder, methylcellulose, starch, polyvinyl alcohol, and polyacrylamide.

5. The preparation method according to any one of claims 1-3, characterized in that, When drying the molded body, the drying temperature is 80-150℃ and the drying time is 1-8 hours; The roasting time is 0.5–6 hours; The oxygen-containing atmosphere is oxygen or a mixture of oxygen and a carrier gas, wherein the volume content of oxygen in the mixture is 2-15%.

6. A catalyst for heavy oil hydrotreating, characterized in that, It is obtained by the preparation method described in any one of claims 1-5.

7. A method for hydrotreating heavy oil, characterized in that, The heavy oil hydrotreating catalyst described in claim 6 is used.

Citation Information

Patent Citations

  • Method for regenerating inactivated hydrotreating catalyst

    CN102451774A

  • Heavy oil hydrogenation catalyst carrier, catalyst and preparation method thereof

    CN111375437A

  • Method for preparing hydrodemetallization catalyst by using deactivated residual oil hydrogenation catalyst

    CN111905838A