Palladium-modified titanium-iron hydrogen storage alloy and preparation method thereof

By doping palladium into titanium-iron hydrogen storage alloys, the problems of activation difficulties and performance degradation in titanium-iron hydrogen storage alloys have been solved, achieving more efficient hydrogen storage and release and enhancing resistance to poisoning by impurity gases.

CN118207458BActive Publication Date: 2026-11-20WESTERN BAODE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410158381.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-04
Publication Date
2026-11-20
Estimated Expiration
2044-02-04

AI Technical Summary

Technical Problem

Existing titanium-iron hydrogen storage alloys suffer from difficulties in activation and performance degradation after repeated hydrogen absorption and desorption.

Method used

By doping palladium into titanium-iron hydrogen storage alloy, Pd²⁺ ions are alloyed with the titanium-iron hydrogen storage alloy during ball milling, replacing some of the lattice positions of Ti and Fe, forming more defects and catalytic sites, and promoting the reversibility of hydrogen and the ability to resist poisoning by impurity gases.

Benefits of technology

It reduces the activation difficulty of titanium-iron hydrogen storage alloys, enhances their reusability and resistance to impurity gas poisoning, and optimizes hydrogen storage and release performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118207458B_ABST
    Figure CN118207458B_ABST
Patent Text Reader

Abstract

The application provides a palladium-modified titanium-iron hydrogen storage alloy and a preparation method thereof, and belongs to the technical field of hydrogen storage alloys. The method comprises the following steps: placing titanium-iron alloy powder and palladium chloride powder in a ball mill tank, adding anhydrous ethanol and grinding balls, performing ball milling after vacuumizing, and obtaining the palladium-titanium-iron hydrogen storage alloy after cleaning and drying. The application provides a palladium-modified titanium-iron hydrogen storage alloy and a preparation method thereof, and realizes the purposes of reducing the activation difficulty of the titanium-iron hydrogen storage alloy, enhancing the reusable capacity and the anti-poisoning capacity to impurity gases.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of hydrogen storage alloy technology, specifically to a palladium-modified titanium-iron hydrogen storage alloy and its preparation method. Background Technology

[0002] With global warming and environmental changes, the development and use of renewable and clean energy is urgently needed, and hydrogen energy, as a secondary clean energy source, has received significant attention. Global energy is accelerating its transition to green and low-carbon practices, and the hydrogen energy industry is developing rapidly. Hydrogen storage and transportation are key nodes, leading to a growing demand for energy storage systems with high energy density, low cost, and high safety. High-pressure gaseous hydrogen storage and transportation, liquid hydrogen storage and transportation, and solid metal hydrides are currently the most common storage and transportation methods. Unlike physical hydrogen storage methods such as high-pressure gas cylinders or cryogenic liquefaction, hydrogen storage alloys store hydrogen in the form of metal hydrides through a chemical reaction with hydrogen, and can release the hydrogen under certain conditions. Using hydrogen storage alloys not only offers advantages such as low energy consumption and ease of use, but also provides a larger hydrogen storage capacity per unit volume compared to the other two methods, eliminating the need for bulky and cumbersome steel containers, making storage and transportation more convenient and safer.

[0003] Common hydrogen storage alloys can be mainly classified into the following categories: AB5 type (rare earth based), AB2 type (zirconium and titanium based), AB type (titanium iron based), A2B type (magnesium based hydrogen storage alloys), and V-based solid solution alloys. AB-type hydrogen storage alloys have attracted widespread attention due to the readily available and abundant raw materials of Ti and Fe metals, and their theoretical hydrogen storage capacity of up to 1.86%. Articles published in the October 2022 issue of the journal *Functional Materials of Metals*, titled "Research on the Modification of AB-type Solid Hydrogen Storage Alloy TiFe," and the August 2019 issue of the *Chinese Journal of Rare Earths*, titled "Research on Easily Activated TiFe-based Hydrogen Storage Alloys," mention that while iron-titanium based hydrogen storage alloys possess advantages such as safety and high efficiency, they also suffer from drawbacks such as difficulty in activation and susceptibility to hydrogenation deactivation.

[0004] Therefore, there is a need to provide a method for preparing titanium-iron hydrogen storage alloys to solve the problems of activation difficulties and performance degradation after repeated hydrogen absorption and desorption in titanium-iron hydrogen storage alloys. Summary of the Invention

[0005] In view of this, the present invention provides a palladium-modified titanium-iron hydrogen storage alloy and its preparation method, which aims to reduce the difficulty of activating titanium-iron hydrogen storage alloy, enhance its reusability and resistance to poisoning by impurity gases.

[0006] To achieve the above objectives, the present invention provides a method for preparing palladium-modified titanium-iron hydrogen storage alloy, comprising the following steps: placing titanium-iron alloy powder and palladium chloride powder in a ball mill jar, adding anhydrous ethanol and grinding balls, ball milling under vacuum, and then cleaning and drying to obtain palladium-titanium-iron hydrogen storage alloy.

[0007] The technical solution provided by this invention employs a simple process that is easy to scale up for production. It utilizes palladium doping (Pd) to achieve this. 2+ During ball milling, ions alloy with the titanium-iron hydrogen storage alloy, replacing some of the lattice positions of Ti and Fe. Because the atomic orbitals of Pd are larger than those of Ti and Fe, the lattice expands, increasing the unit cell volume and forming more defects, which facilitates hydrogen diffusion in the bulk phase and reduces the activation difficulty of the titanium-iron hydrogen storage alloy. Nano-sized palladium chloride, as an alloying element, can make the doping more uniform and form catalytic sites, promoting the reversibility of hydrogen adsorption and desorption in the alloy and enhancing its reusability. Palladium has good catalytic properties and anti-poisoning properties, which can enhance the titanium-iron hydrogen storage alloy's resistance to poisoning by impurity gases.

[0008] Optionally, the mass ratio of the titanium-iron alloy powder to the palladium chloride powder is 1:0.02~0.1.

[0009] Optionally, the purity of the palladium chloride powder is ≥99.99%, and the size of the palladium chloride powder is in the nanometer range.

[0010] Optionally, the volume ratio of the grinding balls to the raw materials is 2:1, and the mass ratio of the raw materials to anhydrous ethanol is 1:5~10.

[0011] Optionally, the ball milling speed is 200~800 r / min, and the ball milling time is 4~20h.

[0012] Optionally, the preparation method of the titanium-iron alloy powder includes taking titanium raw materials and iron raw materials, placing them in a zirconium oxide crucible, and melting the metal by vacuum arc heating to obtain titanium-iron alloy.

[0013] Optionally, the atomic ratio of the titanium raw material to the iron raw material is 1:X, and the chemical formula of the titanium-iron alloy is Ti1Fe. X The range of X is 0 < X ​​≤ 1.

[0014] Optionally, the purity of the titanium raw material and the iron raw material is ≥99.99%.

[0015] Optionally, the cleaning and drying process includes washing three times with anhydrous ethanol and drying in a vacuum drying oven at 50-70°C for 1-4 hours.

[0016] To achieve the above objectives, the present invention also provides a palladium-modified titanium-iron hydrogen storage alloy, which has easy activation and stable hydrogen storage and release capabilities.

[0017] The above-described technical solution of the present invention has at least the following beneficial effects: This invention provides a palladium-modified titanium-iron hydrogen storage alloy and its preparation method, which optimizes the hydrogen storage and release performance of the hydrogen storage alloy, reduces the activation difficulty of existing titanium-iron hydrogen storage alloys, enhances the stability of titanium-iron hydrogen storage alloys, and has a simple process that is easy to scale up for production. Attached Figure Description

[0018] Figure 1 5% Pd-Ti1Fe prepared in Example 1 of this invention 0.9 Ti1Fe prepared in Comparative Example 1 0.9 XRD patterns of hydrogen storage alloys; Figure 2 5% Pd-Ti1Fe prepared in Example 1 of this invention 0.9 Ti1Fe prepared in Comparative Example 1 0.9 PCT curve of hydrogen storage alloy. Detailed Implementation

[0019] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the following will be described in conjunction with the accompanying drawings of the embodiments of the present invention. Figure 1-2 The technical solutions of the embodiments of the present invention will be clearly and completely described herein. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. All other embodiments obtained by those skilled in the art based on the described embodiments of the present invention are within the scope of protection of the present invention.

[0020] Example 1 Titanium and iron metal blocks were prepared with an atomic ratio of 1:0.9. The prepared materials were placed in a zirconium oxide crucible, argon gas was introduced, and a vacuum was created, repeated three times to ensure complete removal of oxygen. The metal materials were then melted using an electric arc to obtain Ti1Fe. 0.9 Hydrogen storage alloy. The hydrogen storage alloy was mechanically crushed to obtain hydrogen storage alloy powder. 250 g of alloy powder and 21.38 g of palladium chloride powder were weighed and placed into a nylon ball mill jar. 20 wt% anhydrous ethanol was added as a solvent, and zirconia grinding balls were added at a ball-to-material volume ratio of 2:1. The jar was sealed, argon gas was introduced, and a vacuum was drawn to below 10 Pa, repeated three times to ensure complete removal of oxygen. The ball milling speed was set to 400 r / min, and the milling time was 8 h. The mixed alloy powder was removed, washed three times with anhydrous ethanol, and dried in a vacuum drying oven at 60 ℃ for 4 h to obtain 5% Pd-Ti1Fe. 0.9 Hydrogen storage alloy.

[0021] X-ray diffraction experiments were performed on the prepared hydrogen storage alloy, and the XRD characterization results are shown in the figure. Figure 1 The prepared hydrogen storage alloy was subjected to PCT testing under the following conditions: temperature: 313 K, activation pressure: 4 MPa. The PCT test results are shown below. Figure 2 .

[0022] The technical solution provided by this invention employs a simple process that is easy to scale up for production. It utilizes palladium doping (Pd) to achieve this. 2+ During ball milling, ions alloy with the titanium-iron hydrogen storage alloy, replacing some of the lattice positions of Ti and Fe. Because the atomic orbitals of Pd are larger than those of Ti and Fe, the lattice expands, increasing the unit cell volume and forming more defects, which facilitates hydrogen diffusion in the bulk phase and reduces the activation difficulty of the titanium-iron hydrogen storage alloy. Nano-sized palladium chloride, as an alloying element, can make the doping more uniform and form catalytic sites, promoting the reversibility of hydrogen adsorption and desorption in the alloy and enhancing its reusability. Palladium has good catalytic properties and anti-poisoning properties, which can enhance the titanium-iron hydrogen storage alloy's resistance to poisoning by impurity gases.

[0023] Example 2 Titanium and iron metal blocks were prepared with an atomic ratio of 1:0.2. The prepared materials were placed in a zirconium oxide crucible, argon gas was introduced, and a vacuum was created, repeated three times to ensure complete removal of oxygen. The metal materials were then melted using an electric arc to obtain Ti1Fe. 0.2 Hydrogen storage alloy. The hydrogen storage alloy was mechanically crushed to obtain hydrogen storage alloy powder. 250 g of alloy powder and 21.38 g of palladium chloride powder were weighed and placed into a nylon ball mill jar. 20 wt% anhydrous ethanol was added as a solvent, and zirconia grinding balls were added at a ball-to-material volume ratio of 2:1. The jar was sealed, argon gas was introduced, and a vacuum was drawn to below 10 Pa, repeated three times to ensure complete removal of oxygen. The ball milling speed was set to 400 r / min, and the milling time was 8 h. The mixed alloy powder was removed, washed three times with anhydrous ethanol, and dried in a vacuum drying oven at 60 ℃ for 2 h to obtain 5% Pd-Ti1Fe. 0.2 Hydrogen storage alloy.

[0024] Example 3 Titanium and iron metal blocks were prepared with an atomic ratio of 1:0.9. The prepared materials were placed in a zirconium oxide crucible, argon gas was introduced, and a vacuum was created, repeated three times to ensure complete removal of oxygen. The metal materials were then melted using an electric arc to obtain Ti1Fe. 0.9 Hydrogen storage alloy. The hydrogen storage alloy was mechanically crushed to obtain hydrogen storage alloy powder. 250 g of alloy powder and 41.67 g of palladium chloride powder were weighed and placed into a nylon ball mill jar. 20 wt% anhydrous ethanol was added as a solvent, and zirconia grinding balls were added at a ball-to-material volume ratio of 2:1. The jar was sealed, argon gas was introduced, and a vacuum was drawn to below 10 Pa, repeated three times to ensure complete removal of oxygen. The ball milling speed was set to 400 r / min, and the milling time was 8 h. The mixed alloy powder was removed, washed three times with anhydrous ethanol, and dried in a vacuum drying oven at 60 ℃ for 3 h to obtain 10% Pd-Ti1Fe. 0.9Hydrogen storage alloy.

[0025] Example 4 Titanium and iron metal blocks were prepared with an atomic ratio of 1:0.9. The prepared materials were placed in a zirconium oxide crucible, argon gas was introduced, and a vacuum was created, repeated three times to ensure complete removal of oxygen. The metal materials were then melted using an electric arc to obtain Ti1Fe. 0.9 Hydrogen storage alloy. The hydrogen storage alloy was mechanically crushed to obtain hydrogen storage alloy powder. 250 g of alloy powder and 8.34 g of palladium chloride powder were weighed and placed in a nylon ball mill jar. 20 wt% anhydrous ethanol was added as a solvent, and zirconia grinding balls were added at a ball-to-material volume ratio of 2:1. The jar was sealed, argon gas was introduced, and a vacuum was drawn to below 10 Pa, repeated three times to ensure complete removal of oxygen. The ball milling speed was set to 400 r / min, and the milling time was 8 h. The mixed alloy powder was removed, washed three times with anhydrous ethanol, and dried in a vacuum drying oven at 60 ℃ for 4 h to obtain 2% Pd-Ti1Fe. 0.9 Hydrogen storage alloy.

[0026] Example 5 Titanium and iron metal blocks were prepared with an atomic ratio of 1:0.5. The prepared materials were placed in a zirconium oxide crucible, argon gas was introduced, and a vacuum was created, repeated three times to ensure complete removal of oxygen. The metal materials were then melted using an electric arc heater to obtain Ti1Fe. 0.5 Hydrogen storage alloy. The hydrogen storage alloy was mechanically crushed to obtain hydrogen storage alloy powder. 250 g of alloy powder and 21.38 g of palladium chloride powder were weighed and placed into a nylon ball mill jar. 10 wt% anhydrous ethanol was added as a solvent, and zirconia grinding balls were added at a ball-to-material volume ratio of 2:1. The jar was sealed, argon gas was introduced, and a vacuum was drawn to below 10 Pa, repeated three times to ensure complete removal of oxygen. The ball milling speed was set to 800 r / min, and the milling time was 4 h. The mixed alloy powder was removed, washed three times with anhydrous ethanol, and dried in a vacuum drying oven at 50 ℃ for 4 h to obtain 5% Pd-Ti1Fe. 0.5 Hydrogen storage alloy.

[0027] Example 6 Titanium and iron metal blocks were prepared with an atomic ratio of 1:0.5. The prepared materials were placed in a zirconium oxide crucible, argon gas was introduced, and a vacuum was created, repeated three times to ensure complete removal of oxygen. The metal materials were then melted using an electric arc heater to obtain Ti1Fe. 0.5Hydrogen storage alloy. The hydrogen storage alloy was mechanically crushed to obtain hydrogen storage alloy powder. 250 g of alloy powder and 21.38 g of palladium chloride powder were weighed and placed into a nylon ball mill jar. 10 wt% anhydrous ethanol was added as a solvent, and zirconia grinding balls were added at a ball-to-material volume ratio of 2:1. The jar was sealed, argon gas was introduced, and a vacuum was drawn to below 10 Pa, repeated three times to ensure complete removal of oxygen. The ball milling speed was set to 200 r / min, and the milling time was 20 h. The mixed alloy powder was removed, washed three times with anhydrous ethanol, and dried in a vacuum drying oven at 70 ℃ for 1 h to obtain 5% Pd-Ti1Fe. 0.5 Hydrogen storage alloy.

[0028] Comparative Example 1 Titanium and iron metal blocks were prepared with an atomic ratio of 1:0.9. The prepared materials were placed in a zirconium oxide crucible, argon gas was introduced, and a vacuum was created, repeated three times to ensure complete removal of oxygen. The metal materials were then melted using an electric arc to obtain Ti1Fe. 0.9 Hydrogen storage alloy. The hydrogen storage alloy was mechanically crushed to obtain hydrogen storage alloy powder. 250 g of the alloy powder was weighed and placed into a nylon ball mill jar. 20 wt% anhydrous ethanol was added as a solvent, and zirconia grinding balls were added at a ball-to-powder volume ratio of 2:1. The jar was sealed, argon gas was introduced, and a vacuum was drawn to below 10 Pa, repeated three times to ensure that oxygen was completely removed. The ball milling speed was set to 400 r / min, and the milling time was 8 h. The mixed alloy powder was taken out, washed three times with anhydrous ethanol, and dried in a vacuum drying oven at 60 ℃ for 4 h to obtain Ti1Fe. 0.9 Hydrogen storage alloy.

[0029] For the prepared Ti1Fe 0.9 X-ray diffraction experiments were performed on the hydrogen storage alloy, and the XRD characterization results are shown in the figure. Figure 1 For the prepared Ti1Fe 0.9 The hydrogen storage alloy underwent PCT testing under the following conditions: temperature 313 K, activation pressure 4 MPa. The PCT test results are shown below. Figure 2 .

[0030] 5% Pd-Ti1Fe prepared in Example 1 0.9 Hydrogen storage alloy and Ti1Fe prepared in Comparative Example 1 0.9 The only difference in the hydrogen storage alloy is that palladium was not added in Comparative Example 1. Figure 1 The results showed that comparing the characteristic peaks of both with those of iron(III) oxide and TiFe revealed that Ti1Fe... 0.9 Hydrogen storage alloys compared to 5% Pd-Ti1Fe 0.9The alloy is severely oxidized, and Pd doping enhances the lattice diffraction peaks of the TiFe alloy phase. Pd doping increases the cell volume, leading to a greater atomic distance between Ti and H atoms after hydrogen absorption. This reduces the attraction of Ti atoms to hydrogen atoms, improving activation performance and facilitating hydrogen release. Furthermore, it weakens the bonding between hydrogen and the primary hydrogen-absorbing Ni atom, making hydrogen extraction easier and thus lowering the hydrogen release temperature.

[0031] 5% Pd-Ti1Fe prepared in Example 1 0.9 Hydrogen storage alloy and Ti1Fe prepared in Comparative Example 1 0.9 The only difference in the hydrogen storage alloy is that palladium was not added in Comparative Example 1. Figure 2 The display shows 5% Pd-Ti1Fe 0.9 The hydrogen storage capacity of the alloy is comparable to that of Ti1Fe. 0.9 There has been a significant improvement. At the same time, the effective hydrogen release capacity has also increased.

[0032] The above are preferred embodiments of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for preparing a palladium-modified titanium-iron hydrogen storage alloy, characterized in that, The process includes the following steps: placing titanium-iron alloy powder and palladium chloride powder in a ball mill jar, adding anhydrous ethanol and grinding balls, ball milling under vacuum, and then cleaning and drying to obtain a palladium-titanium-iron hydrogen storage alloy; the mass ratio of the titanium-iron alloy powder to the palladium chloride powder is 1:0.02~0.1; the volume ratio of the grinding balls to the raw materials is 2:1; and the mass ratio of the raw materials to anhydrous ethanol is 1:5~10.

2. The method for preparing palladium-modified titanium-iron hydrogen storage alloy according to claim 1, characterized in that, The purity of the palladium chloride powder is ≥99.99%, and the size of the palladium chloride powder is in the nanometer range.

3. The method for preparing palladium-modified titanium-iron hydrogen storage alloy according to claim 1, characterized in that, The ball milling speed is 200 ~ 800 r / min, and the ball milling time is 4 ~ 20 h.

4. The method for preparing palladium-modified titanium-iron hydrogen storage alloy according to claim 1, characterized in that, The method for preparing the titanium-iron alloy powder includes taking titanium raw materials and iron raw materials, placing them in a zirconium oxide crucible, and melting the metal by vacuum arc heating to obtain a titanium-iron alloy.

5. The method for preparing palladium-modified titanium-iron hydrogen storage alloy according to claim 4, characterized in that, The atomic ratio of the titanium raw material to the iron raw material is 1:X, the chemical formula of the titanium-iron alloy is Ti1FeX, and the range of X is 0 < X ​​≤ 1.

6. The method for preparing palladium-modified titanium-iron hydrogen storage alloy according to claim 4, characterized in that, The purity of the titanium raw material and the iron raw material is ≥99.99%.

7. The method for preparing palladium-modified titanium-iron hydrogen storage alloy according to claim 1, characterized in that, The cleaning and drying process includes washing three times with anhydrous ethanol and drying in a vacuum drying oven at 50-70°C for 1-4 hours.