Preparation method and application of high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening property

By optimizing the rotary forging process and heat treatment methods, refining the Ni₃Ta phase, and forming twinned and subcrystalline structures, the problem of uneven deformation in traditional tungsten-nickel-iron alloys during rotary forging was solved, resulting in a high-strength and high-self-sharpening tungsten-tantalum-nickel-iron-copper alloy suitable for armor-piercing projectile core materials.

CN118207492BActive Publication Date: 2026-11-24CENT SOUTH UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410316790.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-20
Publication Date
2026-11-24
Estimated Expiration
2044-03-20

AI Technical Summary

Technical Problem

Traditional tungsten-nickel-iron alloys as core materials for armor-piercing projectiles cannot meet the performance requirements of modern warfare, and the rotary forging process cannot effectively improve its thermal shear sensitivity, resulting in uneven deformation of the projectile during penetration, which easily forms a mushroom head and causes kinetic energy loss.

Method used

By designing appropriate rotary forging processes and heat treatment methods, including high-temperature heating, rotary forging, furnace cooling, and low-temperature heating, the Ni₃Ta phase can be refined to form twinned and subcrystalline structures, thereby improving the alloy's adiabatic shear sensitivity.

Benefits of technology

It achieves the self-sharpening capability of high-strength tungsten-tantalum-nickel-iron-copper alloy, improving self-sharpening and strength during penetration, and is suitable for core materials of large-caliber kinetic energy penetrators.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118207492B_ABST
    Figure CN118207492B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing and applying a high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties. The method includes: first, subjecting alloy bars to N-stage rotary forging; then, placing the alloy in a vacuum muffle furnace at 700–900°C for high-temperature heat treatment followed by furnace cooling; and finally, performing low-temperature heat treatment at 400–500°C followed by furnace cooling to obtain the finished product. During the N-stage rotary forging process, the deformation in each stage is 1–4.5%, and high-temperature stress relief treatment is required. This invention ensures that the twinned structures in the binder phase and Ni3Ta phase, as well as the subcrystalline structures in the tungsten particles, remain stable at room temperature while maintaining the coherent relationship between the phase interfaces. The tungsten-tantalum-nickel-iron-copper alloy prepared by this invention possesses high strength and excellent thermal shear sensitivity. As an armor-piercing projectile material, it can achieve "self-sharpening" during high-speed penetration, significantly improving its penetration capability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of tungsten alloy preparation, specifically to a method for preparing and applying a high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties. Background Technology

[0002] Traditional tungsten-nickel-iron alloys prepared by liquid-phase sintering are widely used in armor-piercing projectile core materials due to their excellent strength, hardness, and comprehensive mechanical properties. However, with the development of modern warfare, traditional tungsten-nickel-iron alloys can no longer meet the performance requirements of armor-piercing projectile core materials. Therefore, this paper (202211020238.1) describes a high-strength, ultrafine-grained tungsten-tantalum-nickel-iron-copper alloy, its preparation method, and its application. By designing the material composition system and preparation process, and utilizing the effects of solid solution strengthening, grain refinement strengthening, and second-phase strengthening, a tungsten-tantalum-nickel-iron-copper alloy is prepared with ultimate tensile strength and ultimate compressive strength reaching 1.1 GPa and 1.9 GPa, respectively, which are 30% and 25% higher than those of traditional tungsten-nickel-iron alloys, making it better suited for armor-piercing projectile core materials.

[0003] However, when an armor-piercing projectile penetrates a target plate, the projectile's head is forced to rotate outwards under axial force, forming a larger "mushroom head" that increases the force-bearing area and causes additional kinetic energy loss, severely affecting penetration. To maximize the penetration capability of tungsten-tantalum-nickel-iron-copper alloy as the core material of an armor-piercing projectile, it is necessary to enhance the adiabatic shear sensitivity of the prepared high-strength tungsten-tantalum-nickel-iron-copper alloy, allowing the projectile to continuously "self-sharpen" during penetration, enabling it to penetrate the target with a sharper projectile posture and improving penetration capability.

[0004] Rotary forging, as a conventional deformation strengthening process, can increase the dislocation density within the alloy, thereby reducing the critical strain for the formation of adiabatic shear bands, increasing adiabatic shear sensitivity, and enhancing the "self-sharpening" ability during penetration. However, the tungsten-tantalum-nickel-iron-copper alloy prepared by 202211020238.1 contains a nano-Ni3Ta strengthening phase with extremely high hardness and excellent toughness. The high hardness of the strengthening phase leads to uneven deformation of the alloy during rotary forging, causing changes in grain orientation and resulting in uneven mechanical properties in different directions. Furthermore, under the high temperature and high strain conditions of rotary forging, the strengthening phase may dissolve or redistribute, leading to brittle fracture or crack propagation during deformation. These factors prevent traditional rotary forging processes from achieving deformation strengthening of tungsten-tantalum-nickel-iron-copper alloys and improving their adiabatic shear sensitivity.

[0005] The main feature of this patent is that, while ensuring the high strength of the tungsten-tantalum-nickel-iron-copper alloy, a high-strength tungsten-tantalum-nickel-iron-copper alloy is obtained by designing a suitable rotary forging process, and then applied to the core material of armor-piercing projectiles. Summary of the Invention

[0006] This invention addresses the problems of uneven deformation, dissolution and redistribution of strengthening phases, crack propagation, and brittle fracture in nano-Ni3Ta-reinforced tungsten-tantalum-nickel-iron-copper alloys during rotary forging. The first objective of this invention is to provide a method for preparing a high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties. This alloy exhibits higher strength, superior thermal shear sensitivity, and better "self-sharpening" ability during penetration.

[0007] The second objective of this invention is to provide an application of the high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties prepared by the above-described preparation method.

[0008] To achieve the above objectives, the present invention provides the following technical solution: This invention discloses a method for preparing a self-sharpening high-strength tungsten-tantalum-nickel-iron-copper alloy, comprising rotary forging and heat treatment. The tungsten-tantalum-nickel-iron-copper alloy rod is first heated to a high temperature of 800-1300℃ in a vacuum muffle furnace, then placed in a rotary forging device for N-stage rotary forging. After rotary forging, the alloy is placed in a vacuum muffle furnace at 700-900℃ for high-temperature heat treatment followed by furnace cooling, and then subjected to low-temperature heat treatment at 400-500℃ followed by furnace cooling to obtain the finished product. After each stage of rotary forging, the tungsten-tantalum-nickel-iron-copper alloy is held at 700-900℃ in a vacuum muffle furnace for 5-30 minutes, then heated to a rotary forging temperature of 800-1300℃ and held for 10-30 minutes before proceeding to the next stage of rotary forging.

[0009] Preferably, the original sample of the tungsten-tantalum-nickel-iron-copper alloy used in this invention is a sample selected from patent 202211020238.1. Its composition consists of (tungsten + tantalum), nickel, iron, and copper in a mass ratio of (tungsten + tantalum):nickel:iron:copper = 90:3.5~6.3:1.5~2.7:1~5; wherein the mass ratio of tungsten to tantalum is 85~95:5~15.

[0010] The preparation method of the original tungsten-tantalum-nickel-iron-copper alloy sample includes powder metallurgy, preferably the preparation method of patent 202211020238.1.

[0011] As a further preferred embodiment, the original tungsten-tantalum-nickel-iron-copper alloy sample in this invention was obtained using the materials and preparation process selected in Example 1 of document 202211020238.1. That is: A method for preparing a low-temperature sintered high-strength ultrafine-grained tungsten-tantalum-nickel-iron-copper alloy includes the following steps: Step 1: Prepare tungsten-tantalum pre-alloyed powder using mechanical alloying; Take 171g of tungsten powder with an average particle size of 3-5μm and a purity greater than 99.8%; and 9g of tantalum powder with an average particle size of 30μm and a purity greater than 99.5%. Place the tungsten powder and tantalum powder into a tungsten carbide ball mill jar and add anhydrous ethanol to half the jar's volume. Add 1800g of tungsten carbide balls with a diameter of 6mm. Seal the ball mill jar and introduce high-purity argon gas through a vent valve. Perform the ball milling experiment using a QXQM-16 omnidirectional planetary ball mill for 60 hours at a speed of 300 rpm / min. After ball milling, pour the tungsten-tantalum pre-alloyed powder and anhydrous ethanol into a tray and place it in a vacuum glove box in a high-temperature drying oven for drying at 50℃ for 40 hours. The dried tungsten-tantalum pre-alloyed powder was transferred into a GSL-1200X-II high-temperature vacuum tube furnace, and high-purity hydrogen was introduced at a rate of 0.5 L / min for 30 min before heating began. The temperature was first increased to 600°C at a rate of 10°C / min and held for 2 h; then increased to 900°C at a rate of 5°C / min and held for 0.5 h; and finally cooled to room temperature at a rate of 10°C / min to obtain the tungsten-tantalum pre-alloyed powder.

[0012] Step 2: Preform Preparation Process Take 180g of tungsten-tantalum pre-alloyed powder; 9.8g of nickel powder with an average particle size of 3-5μm and a purity greater than 99.9%; 4.2g of iron powder with an average particle size of 3-5μm and a purity greater than 99.5%; and 6g of copper powder with an average particle size of 3-5μm and a purity greater than 99.8%. Put all the powders into a three-dimensional mixer and mix for 12 hours. After mixing, put the mixed powder into a rubber sleeve and place it in a cold isostatic pressing furnace for cold pressing at a pressure of 250MPa to obtain a pressed blank.

[0013] Step 3: Sintering of tungsten-tantalum-nickel-iron-copper alloy The sintering process used a VVP-60 vacuum hot pressing sintering furnace from Shanghai Haoyue Electric Furnace Technology Co., Ltd.; during the sintering process, the vacuum level inside the furnace was maintained at 10. -3 Below Pa; first, heat to 900℃ at a rate of 10℃ / min and hold for 0.5h; then heat to 1350℃ at a rate of 5℃ / min and hold for 1h; then cool to 1100℃ at a rate of 10℃ / min and hold for 3h; finally cool to room temperature at a rate of 10℃ / min to complete the sintering process and obtain a high-strength tungsten-tantalum-nickel-iron-copper alloy.

[0014] The average density of the tungsten-tantalum-nickel-iron-copper alloy is 16.75 g / cm³. 3 The average relative density is 97.89%, the average elongation is 17.11%, the average tensile strength is 1100 MPa, the average compressive yield strength is 1300 MPa, the average compressive ultimate strength is 1600 MPa, and the average grain size is 6.83 μm.

[0015] Preferably, the rotary forging process of this invention is as follows: tungsten-tantalum-nickel-iron-copper alloy bars are placed in a vacuum muffle furnace for high-temperature heating, with a vacuum degree ≤1×10⁻⁶. -3 Pa, setting the heating rate to 15~35℃ / min, the temperature to 800~1300℃, preferably 900~1150℃, further preferably 950~1100℃, and even more preferably 980~1020℃, and holding for 10~30min; then placing it in a rotary forging machine, setting the rotary forging frequency to 800~1500 times / min, the rotary forging deformation amount in each stage to 1~4.5%, and performing rotary forging in N stages (N≥1), with a total rotary forging deformation amount of 20~70%.

[0016] As a further preferred option, the amount of forging deformation per stage is 1.5~3.5%, even more preferably 1.5~3%, and even more preferably 1.8~2.2%, which of course includes 2.0%, 2.1%, 1.9%, etc.

[0017] As a further preferred option, the total deformation of rotary forging is 30-55%, even more preferably 30-50%, and still even more preferably 38-42%; this range naturally includes 39%, 40%, 41%, etc.

[0018] As a further preferred option, the forging frequency is 1000~1300 times / minute, even more preferably 1150~1250 times / minute, and even more preferably 1180~1220 times / minute. This range naturally includes 1200 times / minute, 1180 times / minute, 1190 times / minute, 1210 times / minute, 1220 times / minute, etc.

[0019] The inventors discovered that forging temperature, forging frequency, deformation amount per stage, and total forging deformation have a significant impact on material properties. For tungsten-tantalum-nickel-iron-copper alloys, when the forging temperature exceeds 1200℃, the liquidus temperature of the binder phase is 1350℃, leading to localized compositional segregation and thermal fluctuations during high-speed rotary forging. When the forging temperature is below 900℃, the alloy does not soften, and the high-hardness alloy cannot be deformed through rotary forging. Simultaneously, the Ni3Ta phase readily merges and grows, accumulating during high-speed rotary forging and reducing alloy properties. When the forging frequency exceeds 1200 cycles / minute, the forging speed is too fast, exceeding the toughness limit of the tungsten particles. This leads to micropores within the tungsten particles, which develop into cracks, ultimately causing material fracture. When the forging frequency is below 900 cycles / minute, the forging speed is too low to provide and transmit sufficient stress to the alloy's interior. This prevents the formation of twin structures in the binder phase, and subgrain structures within the tungsten particles are also unattainable. Instead, high-density dislocations form in both the binder phase and the tungsten particles. This is because during forging, the alloy is subjected to high strain rates and strain gradients, causing lattice deformation and movement. Rapid strain and strain gradients trigger grain boundary migration and dislocation movement within the crystal, thus promoting the formation of twins and subgrains. Furthermore, the energy at the alloy grain boundaries increases during deformation, promoting grain boundary migration and recrystallization. Because twins and subgrains have high surface and internal energy, these structures are more likely to form at grain boundaries or in regions where dislocations accumulate. When the forging temperature or frequency is too low, it is impossible to create complex hot deformation conditions within the alloy, and high strain rate and strain gradient cannot be achieved. Furthermore, when the deformation per stage exceeds 3%, the significant differences in hardness and toughness among the tungsten particles, binder phase, and Ni3Ta phase lead to uneven deformation within the alloy, potentially even causing tungsten particles to break. Conversely, when the deformation per stage is less than 1%, the insufficient deformation results in high energy consumption and equipment wear, increasing processing costs. When the total rotary forging deformation exceeds 50%, a large number of subgrains or even recrystallizations form inside the binder phase, and recrystallized grains also precipitate at the phase interface. Furthermore, due to the excessively high rotary forging deformation, the internal stress of the material is extremely high and cannot be effectively eliminated, resulting in a large number of crack initiation sites inside the alloy during high-speed penetration, and a significant decrease in alloy performance. When the total rotary forging deformation is less than 30%, the microstructure of the binder phase mainly exists in the form of dislocation walls and dislocation cells, and the tungsten particles are also mainly composed of dislocation entanglements. This is because the total deformation is too small, and the frictional heat and thermal deformation generated by plastic deformation during the rotary forging process are insufficient, which cannot promote the recrystallization and dynamic recovery of the crystals, thereby generating new grain boundaries and subgrain structures. At this time, the improvement effect on the overall strength and thermal shear sensitivity of the alloy is limited.

[0020] Further preferably, during the rotary forging process, the vacuum degree is ≤1×10⁻⁶. -3 Pa, the vacuum muffle furnace heating rate is 20~30℃ / min, and the holding time is 10~30min, preferably 15~25min.

[0021] Because the Ni3Ta phase in the original tungsten-tantalum-nickel-iron-copper alloy sample was unevenly distributed, the high hardness and toughness of the Ni3Ta phase after rotary forging caused uneven deformation of the alloy. Simultaneously, the Ni3Ta phase became elongated and flattened, and some Ni3Ta phases accumulated and formed clusters, resulting in the alloy's performance not achieving the desired improvement. This invention, through subsequent heat treatment processes, can effectively refine the Ni3Ta phase after rotary forging and homogenize the microstructure. This results in an alloy that, while improving strength, significantly enhances thermal shear sensitivity and greatly improves its self-sharpening ability.

[0022] In this invention, a method for preparing a self-sharpening high-strength tungsten-tantalum-nickel-iron-copper alloy is disclosed. After each stage of rotary forging, the alloy is held at 700-900℃ in a vacuum muffle furnace for 5-30 minutes. This process releases the stress generated during the rotary forging stage; otherwise, the sample is highly susceptible to breakage. After holding at 700-900℃, the alloy can be cooled and then heated back to the rotary forging temperature, or it can be directly heated to the rotary forging temperature.

[0023] Because tungsten-tantalum-nickel-iron-copper alloys contain not only high-melting-point W but also low-melting-point Cu, and the binder phase also contains Ni3Ta, traditional heat treatment methods cannot achieve the desired material properties. Therefore, in a heat treatment method for tungsten-tantalum-nickel-iron-copper alloys (202311357464.3), a high-temperature heating-oil quenching-low-temperature heating-water quenching heat treatment process is designed. This process not only refines the Ni3Ta phase in the binder phase but also maintains the γ-(Ni,Fe,Cu) solid solution phase structure of the binder phase at room temperature, and the binder phase and tungsten particles remain in a good KS coherent interface relationship. Ultimately, a tungsten-tantalum-nickel-iron-copper alloy with significantly improved strength and toughness is obtained.

[0024] In a heat treatment method for a tungsten-tantalum-nickel-iron-copper alloy (202311357464.3), the tungsten-tantalum-nickel-iron-copper alloy is first subjected to high-temperature heat treatment, which causes the Ni3Ta phase to redissolve through solid-state diffusion reaction and exist in the form of a supersaturated solid solution. Oil quenching inhibits the precipitation of the Ni3Ta phase and shortens the time for the Ni3Ta phase to merge and grow, thereby refining the Ni3Ta phase. Then, the tungsten-tantalum-nickel-iron-copper alloy is subjected to low-temperature heat treatment, which causes Cu to redissolve into the binder phase and generate a γ-(Ni,Fe,Cu) phase. Water quenching inhibits the precipitation of Cu in the binder phase and obtains a stable γ-(Ni,Fe,Cu) solid solution phase structure.

[0025] The main feature of the heat treatment process of this invention is that, while ensuring the refinement of the Ni3Ta phase in the tungsten-tantalum-nickel-iron-copper alloy to obtain a stable γ-(Ni,Fe,Cu) solid solution phase structure, it is also necessary to ensure that, after rotary forging, the twin structure formed in the binder phase cuts through different Ni3Ta phases, as well as the subcrystalline structure in the tungsten particles (in this invention, the twin length is very long, so it generally cuts through many different Ni3Ta phases simultaneously). Because the deformation characteristics of traditional tungsten-nickel-iron alloys during penetration change according to the increase in deformation amount, from uniform plastic deformation to adiabatic shear deformation to adiabatic shear failure, the critical values ​​for deformation amount are usually 0~50%, 50%~75%, and above 75%. In the uniform plastic deformation stage, the main characteristic inside the tungsten particles is the appearance of screw dislocations, with dislocation entanglement in the binder phase; in the adiabatic shear deformation stage, the main characteristic inside the tungsten particles is a subcrystalline structure, with a large number of subcrystalline structures or twins forming in the binder phase; in the adiabatic shear failure stage, the main characteristic inside the tungsten particles is a subcrystalline structure, with a large number of recrystallized grains forming in the binder phase. These deformed microstructure characteristics reflect the inherent mechanism of the poor adiabatic shear sensitivity of traditional tungsten-nickel-iron alloys. This is due to the inherent properties of tungsten alloys, which inevitably undergo these microstructural evolutions before adiabatic shear failure can occur. Therefore, tungsten-tantalum-nickel-iron-copper alloys must also undergo these microstructural evolutions. Rotary forging can cause a large number of twins to appear in the Ni3Ta phase and the binder phase in the treated tungsten-tantalum-nickel-iron-copper alloy, while subgrained structures appear in the tungsten particles. This is equivalent to allowing the tungsten-tantalum-nickel-iron-copper alloy to directly skip the uniform plastic deformation stage. In the initial stage of the penetration process, the core material of the tungsten-tantalum-nickel-iron-copper alloy is in the adiabatic shear deformation stage. Therefore, adiabatic shear failure can occur with a smaller amount of deformation, that is, it has better adiabatic shear sensitivity and excellent "self-sharpening" properties.

[0026] This invention first performs high-temperature heat treatment on the tungsten-tantalum-nickel-iron-copper alloy after rotary forging (including each stage of rotary forging and N-stage rotary forging), at 700~900℃, instead of using the 1100~1250℃ temperature range disclosed in 202311357464.3. This is to ensure the stability of the twin structure in the binder phase at a relatively lower heat treatment temperature, while maintaining the effect of refining the Ni3Ta phase after the twins cut through it, and preserving the subgrain structure in the tungsten particles. Furthermore, furnace cooling is preferred after high-temperature heat treatment, rather than immediate oil quenching after high-temperature heat treatment as disclosed in 202311357464.3. This is to prevent excessively rapid cooling. Due to the complex subgrain structure of the tungsten particles in the alloy, the differences in the twin structure of the binder phase, and the refined Ni3Ta phase after the twins cut through it, large thermal stress is generated at the phase interface. Furnace cooling after high-temperature heat treatment effectively solves this problem.

[0027] In this invention, after high-temperature annealing, the alloy is furnace-cooled to 400-500°C for low-temperature heat treatment to obtain a stable γ-(Ni,Fe,Cu) solid solution phase structure. Because furnace cooling is chosen after the high-temperature heat treatment, Cu in the γ-(Ni,Fe,Cu) solid solution phase precipitates during the slow cooling process, and the binder phase transforms into γ-(Ni,Fe)-Cu. x The clustered structure, which lacks coherence with the Ni3Ta phase, leads to a significant decrease in alloy properties. Low-temperature heat treatment at 400–500℃ allows Cu to redissolve and re-enter the binder phase, forming γ-(Ni,Fe)-Cu. x The cluster structure reverts to a γ-(Ni,Fe,Cu) solid solution phase. The process of furnace cooling following low-temperature heat treatment differs from the immediate water quenching after low-temperature heat treatment disclosed in 202311357464.3. This is also to avoid a high cooling rate that could destroy the twin and subgrain structures in the alloy, and to prevent large thermal stresses at the phase interfaces. Furnace cooling also suppresses the re-precipitation of Cu, allowing the binder phase to maintain a stable γ-(Ni,Fe,Cu) solid solution phase structure at room temperature.

[0028] All heat treatment processes in this invention are carried out in a vacuum environment to avoid oxidation of the samples.

[0029] In a preferred embodiment, the heat treatment process is as follows: the forged tungsten-tantalum-nickel-iron-copper alloy is placed in a vacuum muffle furnace, and a vacuum is drawn to achieve a vacuum degree of ≤1×10⁻⁶. -3 The pressure is then increased to 700-900℃ at a heating rate of 10-20℃ / min, held for 5-10 hours, followed by furnace cooling to 400-500℃, held for 1-5 hours, and finally cooled to room temperature (25℃). The vacuum level is maintained at ≤1×10⁻⁶ during heating, holding, and cooling. -2 Pa.

[0030] In the heat treatment process of this invention, during high-temperature heat treatment holding, if the temperature is too high, the Ni3Ta phase cut by twinning is prone to coalescence and growth; if the temperature is too low, the residual stress inside the alloy caused by rotary forging cannot be effectively eliminated. During low-temperature heat treatment holding, if the temperature is too high, the highly oxidizing Ta is prone to secondary oxidation; if the temperature is too low, Cu cannot be redissolved to form a stable γ-(Ni,Fe,Cu) solid solution phase. If the holding time is too long, grain growth will occur; if the holding time is too short, the alloy will be fully heated, failing to achieve the effect of homogenized annealing. In addition, controlling the heating rate during the heating process can stabilize the thermal field in the vacuum muffle furnace and ensure uniform heating of the tungsten-tantalum-nickel-iron-copper alloy during heating.

[0031] Further preferably, the heat treatment process is as follows: the tungsten-tantalum-nickel-iron-copper alloy after each stage of rotary forging is placed in a vacuum muffle furnace, and a vacuum is drawn to achieve a vacuum degree of ≤1×10⁻⁶. -3 Pa, then heated to 750-850℃ at a heating rate of 10-15℃ / min, held for 5-8 hours, followed by furnace cooling to 400-450℃, held for 1-3 hours, and finally furnace cooled to, preferably, room temperature (25℃). The vacuum level must be maintained at ≤1×10⁻⁶ during heating, holding, and cooling. -2 Pa.

[0032] The high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties prepared by the present invention has high strength, fine grains, strong deformation ability, and excellent thermal shear sensitivity, which can meet the extremely high requirements of the field for high strength and high self-sharpening properties of tungsten alloys.

[0033] The present invention also provides the application of the high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties prepared by the above preparation method, and applies the tungsten-tantalum-nickel-iron-copper alloy to the core material of large-caliber kinetic energy penetrators. Beneficial effects

[0034] The rotary forging technique designed in this invention serves as a high-temperature plastic deformation preparation method. The high deformation temperature and strain rate during the rotary forging process can promote the formation of twins within the binder phase and Ni3Ta nano-reinforcing phase of the tungsten-tantalum-nickel-iron-copper alloy, and the formation of subcrystalline structures within the tungsten particles, thereby improving the strength of the material. Furthermore, it enables the tungsten-tantalum-nickel-iron-copper alloy to form an adiabatic shear band with a smaller deformation during high-speed penetration, resulting in a self-sharpening tungsten-tantalum-nickel-iron-copper alloy.

[0035] This invention, by designing appropriate rotary forging process parameters, including rotary forging temperature, rotary forging frequency, rotary forging deformation per stage, and total rotary forging deformation, enables the formation of numerous twinned structures in the binder phase and Ni3Ta phase of the tungsten-tantalum-nickel-iron-copper alloy, and the formation of subcrystalline structures in the tungsten particles, thereby achieving higher strength and hardness. Simultaneously, the self-sharpening tungsten-tantalum-nickel-iron-copper alloy obtained after rotary forging possesses higher internal strain energy. The constructed twinned and subcrystalline structures provide defect nucleation and growth sites for the formation and expansion of adiabatic shear bands, as well as for adiabatic shear failure. This allows the alloy to achieve adiabatic shear failure with a smaller deformation during penetration, providing a beneficial effect on the alloy's "self-sharpening."

[0036] This invention, through a designed heat treatment process—high-temperature heating followed by furnace cooling, then low-temperature heating again followed by furnace cooling—maintains the twin structure in the binder phase by holding the alloy at 750-850℃ for 5-8 hours followed by furnace cooling to 400-450℃. This stabilizes the twin structure and preserves the refinement of the Ni3Ta phase achieved by the twins cutting through it, while also retaining the subgrain structure of the tungsten particles. Further holding the alloy at 400-500℃ for 1-3 hours followed by furnace cooling allows Cu to redissolve and re-enter the binder phase, forming γ-(Ni,Fe)-Cu. x The cluster structure is transformed back into the γ-(Ni,Fe,Cu) solid solution phase, avoiding a large cooling rate that would destroy the twin and subcrystalline structures in the alloy, while also avoiding large thermal stress at the phase interface, thus obtaining a stable γ-(Ni,Fe,Cu) solid solution phase structure at room temperature.

[0037] The high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties prepared by the method of the present invention has, compared with the tungsten-tantalum-nickel-iron-copper alloy provided in Example 1 of 202211020238.1, an increased compressive yield strength of 1.78 GPa to 2.04 GPa, an increased ultimate compressive strength of 1.95 GPa to 2.28 GPa, and a decrease in adiabatic shear failure deformation of 60% to 45%.

[0038] The high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties provided by this invention not only has high strength, but also has significantly higher thermal shear sensitivity than traditional tungsten-nickel-iron alloys. It can be used to manufacture the core of large-caliber kinetic energy penetrators, greatly enhancing the application potential of tungsten alloys.

[0039] This invention is the first to achieve a balance between high strength and high self-sharpening properties in a product. Attached Figure Description

[0040] Figure 1 This is a process flow diagram of the present invention.

[0041] Figure 2 The microstructure of the tungsten-tantalum-nickel-iron-copper alloy obtained by the method in Example 1 is shown.

[0042] Figure 3 The stress-strain curves and nanoindentation hardness data of the tungsten-tantalum-nickel-iron-copper alloy under dynamic compression obtained by the method in Example 1 are shown below; (a) stress-strain curves; (b) nanoindentation hardness data.

[0043] Figure 4 The microstructure of the tungsten-tantalum-nickel-iron-copper alloy obtained by the method of Example 1 after dynamic compression is shown in (a) and (b) the microstructure after dynamic compression deformation of 30%.

[0044] Figure 5 The microstructure of the tungsten-tantalum-nickel-iron-copper alloy obtained by the method in Comparative Example 1 after dynamic compression is shown. Figure 1 The basic process flow of this invention can be seen.

[0045] from Figure 2 It can be seen that the Ni3Ta phase in the rotary forged sample is needle-shaped, with a length of 50~300nm and a width of 1~5nm. The tungsten particles are ellipsoidal, with a long semi-axis particle size of 10~50μm and a short semi-axis particle size of 1~10μm.

[0046] from Figure 3 As can be seen from (a), the dynamic yield strength of the alloy is 2.04 GPa, and the ultimate strength is 2.28 GPa. Figure 3 As can be seen in (b), the hardness of the tungsten particles in the adiabatic shear region is 9.4 GPa, the hardness of the binder phase is 5.8 GPa, and the hardness of the Ni3Ta phase is 15.6 GPa.

[0047] from Figure 4 It can be seen from 10 3 s -1 Under strain rate loading conditions, an adiabatic shear band appears after the deformation reaches 30%, and adiabatic shear failure occurs when the deformation reaches 45%.

[0048] from Figure 5 As can be seen from the comparison, the microstructure of the tungsten-tantalum-nickel-iron-copper alloy obtained by the method of Comparative Example 1 after dynamic compression is similar to that of the product obtained in Example 1. Detailed Implementation

[0049] The composition and preparation method of the tungsten-tantalum-nickel-iron-copper alloy used in this method are as described in Example 1 of 202211020238.1, "A High-Strength Ultrafine-Grained Tungsten-tantalum-nickel-iron-copper Alloy, Its Preparation Method and Application". Example 1

[0050] Step 1: Sample Rotary Forging Process Tungsten-tantalum-nickel-iron-copper alloy rods were placed in a vacuum muffle furnace and heated at high temperature with a vacuum degree ≤1×10⁻⁶. -3 The heating rate was set to 20℃ / min, the temperature to 1000℃, and the holding time to 15min. The workpiece was then placed in a rotary forging machine, with a rotary forging frequency of 1200 times / min. The forging deformation was 2% per stage, and the rotary forging was performed in 20 stages, with a total forging deformation of 40%. After each stage of rotary forging, the workpiece was placed in a vacuum muffle furnace and held at 800℃ for 10min. After holding, the temperature was raised to 1000℃ and held for 15min. The next stage of rotary forging was then performed, and this cycle was repeated until the total forging deformation reached 40%, at which point the rotary forging was complete. The resulting rotary-forged tungsten-tantalum-nickel-iron-copper alloy was obtained. Step 2: Sample heat treatment process The forged tungsten-tantalum-nickel-iron-copper alloy was placed in a vacuum muffle furnace and evacuated to a vacuum level of ≤1×10⁻⁶. -3 Pa, then heated to 800℃ at a heating rate of 10℃ / min, held for 6 hours, followed by furnace cooling to 450℃, held for 1.5 hours, and finally cooled to room temperature (25℃). The vacuum level was maintained at ≤1×10⁻⁶ during heating, holding, and cooling. -2 Pa.

[0051] Figure 2 The morphology of the alloy obtained by the method in Example 1 shows that the Ni3Ta phase in the sample is needle-shaped with a length of 50~300nm and a width of 1~5nm. The tungsten particles are ellipsoidal with a long semi-axis particle size of 10~50μm and a short semi-axis particle size of 1~10μm.

[0052] Figure 3 The stress-strain curves and nanoindentation hardness data of the alloy under dynamic compression obtained by the method in Example 1 show that the dynamic yield strength of the alloy is 2.04 GPa, the ultimate strength is 2.28 GPa, the hardness of the tungsten particles in the adiabatic shear region is 9.4 GPa, the hardness of the binder phase is 5.8 GPa, and the hardness of the Ni3Ta phase is 15.6 GPa.

[0053] Figure 4 The images show the morphology of the alloy obtained by the method in Example 1 during dynamic compression when adiabatic shear deformation and adiabatic shear failure occur. It can be seen that the sample exhibits adiabatic shear deformation when the deformation amount is 30% and adiabatic shear failure when the deformation amount is 45%.

[0054] The performance results of the tungsten-tantalum-nickel-iron-copper alloy obtained in Example 1 are shown in Table 1.

[0055] These test results demonstrate that the tungsten-tantalum-nickel-iron-copper alloy prepared by the method in Example 1 not only has high strength, but also significantly improved thermal shear sensitivity, ultimately resulting in a high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties. Example 2

[0056] Step 1: Sample Rotary Forging Process Tungsten-tantalum-nickel-iron-copper alloy rods were placed in a vacuum muffle furnace and heated at high temperature with a vacuum degree ≤1×10⁻⁶. -3The heating rate was set to 20℃ / min, the temperature to 950℃, and the holding time to 15min. The workpiece was then placed in a rotary forging machine with a forging frequency of 1300 times / min. The forging deformation was 1.5% per stage, and the process was repeated in 30 stages, with a total forging deformation of 45%. After each stage of rotary forging, the workpiece was placed in a vacuum muffle furnace and held at 750℃ for 10min. After holding at 750℃, the temperature was raised to 950℃ and held for 15min. The next stage of rotary forging was then performed, and this cycle was repeated until the total forging deformation reached 45%, at which point the rotary forging was complete. The resulting rotary-forged tungsten-tantalum-nickel-iron-copper alloy was obtained. Step 2: Sample heat treatment process The forged tungsten-tantalum-nickel-iron-copper alloy was placed in a vacuum muffle furnace and evacuated to a vacuum level of ≤1×10⁻⁶. -3 Pa, then heated to 750℃ at a heating rate of 10℃ / min, held for 8 hours, followed by furnace cooling to 400℃, held for 2 hours, and finally cooled to room temperature (25℃). The vacuum level was maintained at ≤1×10⁻⁶ during heating, holding, and cooling. - 2 Pa.

[0057] The performance results of the tungsten-tantalum-nickel-iron-copper alloy obtained in Example 2 are shown in Table 1. Example 3

[0058] Step 1: Sample Rotary Forging Process Tungsten-tantalum-nickel-iron-copper alloy rods were placed in a vacuum muffle furnace and heated at high temperature with a vacuum degree ≤1×10⁻⁶. -3 The heating rate was set to 20℃ / min, the temperature to 1050℃, and the holding time to 15min. The workpiece was then placed in a rotary forging machine, with a rotary forging frequency of 1100 times / min. The forging deformation was 2.5% per stage, and the process was repeated in 20 stages, with a total forging deformation of 50%. After each stage of rotary forging, the workpiece was placed in a vacuum muffle furnace and held at 800℃ for 10min. After holding at 800℃, the temperature was raised to 1050℃ and held for 15min. The next stage of rotary forging was then performed, and this cycle was repeated until the total forging deformation reached 50%, at which point the rotary forging was complete. The resulting rotary-forged tungsten-tantalum-nickel-iron-copper alloy was obtained. Step 2: Sample heat treatment process The forged tungsten-tantalum-nickel-iron-copper alloy was placed in a vacuum muffle furnace and evacuated to a vacuum level of ≤1×10⁻⁶. -3 Pa, then heated to 800℃ at a heating rate of 10℃ / min, held for 5 hours, followed by furnace cooling to 450℃, held for 1 hour, and finally cooled to room temperature (25℃). The vacuum level was maintained at ≤1×10⁻⁶ during heating, holding, and cooling. - 2 Pa.

[0059] The performance results of the tungsten-tantalum-nickel-iron-copper alloy obtained in Example 3 are shown in Table 1. Example 4

[0060] Step 1: Sample Rotary Forging Process Tungsten-tantalum-nickel-iron-copper alloy rods were placed in a vacuum muffle furnace and heated at high temperature with a vacuum degree ≤1×10⁻⁶. -3 The heating rate was set to 20℃ / min, the temperature to 1100℃, and the holding time to 15min. The workpiece was then placed in a rotary forging machine, with a forging frequency of 1000 times / min. The forging deformation was 3% per stage, and the forging was performed in 15 stages, with a total forging deformation of 45%. After each stage of rotary forging, the workpiece was placed in a vacuum muffle furnace and held at 850℃ for 10min. After holding at 850℃, the temperature was raised to 1100℃ and held for 15min. The next stage of rotary forging was then performed, and this cycle was repeated until the total forging deformation reached 45%, at which point the rotary forging was complete. The resulting rotary-forged tungsten-tantalum-nickel-iron-copper alloy was obtained. Step 2: Sample heat treatment process The forged tungsten-tantalum-nickel-iron-copper alloy was placed in a vacuum muffle furnace and evacuated to a vacuum level of ≤1×10⁻⁶. -3 Pa, then heated to 850℃ at a heating rate of 10℃ / min, held for 4.5h, followed by furnace cooling to 450℃, held for 1h, and finally cooled to room temperature (25℃). The vacuum level was maintained at ≤1×10⁻⁶ during heating, holding, and cooling. -2 Pa.

[0061] The performance results of the tungsten-tantalum-nickel-iron-copper alloy obtained in Example 4 are shown in Table 1. Example 5

[0062] The difference from Example 1 is that the forging deformation amount is 2% in each stage, the forging is carried out in 15 stages, the total forging deformation amount is 30%, and the rest of the operations are the same.

[0063] The performance results of the tungsten-tantalum-nickel-iron-copper alloy obtained in Example 5 are shown in Table 1.

[0064] Comparative Example 1 The difference from Example 1 is that the temperature during the rotary forging process is 1200°C, while the rest of the operations are the same.

[0065] Figure 5The images show the morphology of the alloy obtained using the method in Comparative Example 1 during dynamic compression under adiabatic shear deformation and adiabatic shear failure. It can be seen that the sample exhibits adiabatic shear deformation at a deformation amount of 40% and adiabatic shear failure at a deformation amount of 60%. Both deformation amounts are higher than those of the tungsten-tantalum-nickel-iron-copper alloy obtained in Example 1, and the width of the adiabatic shear band in the initial stage of adiabatic shear deformation is also greater than that of the sample in Example 1. These results demonstrate that the tungsten-tantalum-nickel-iron-copper alloy obtained in Comparative Example 1 has poor adiabatic shear sensitivity.

[0066] The performance results of the tungsten-tantalum-nickel-iron-copper alloy obtained in Comparative Example 1 are shown in Table 1.

[0067] Comparative Example 2 The difference from Example 1 is that the deformation amount of rotary forging in each stage of the rotary forging process is 5%, while the rest of the operations are the same.

[0068] The performance results of the tungsten-tantalum-nickel-iron-copper alloy obtained in Comparative Example 2 are shown in Table 1.

[0069] Comparative Example 3 The difference from Example 1 is that the high-temperature heat treatment temperature in the heat treatment process is 1100°C, while the rest of the operations are the same.

[0070] The performance results of the tungsten-tantalum-nickel-iron-copper alloy obtained in Comparative Example 3 are shown in Table 1.

[0071] Comparative Example 4 The difference from Example 1 is that the low-temperature heat treatment temperature in the heat treatment process is 300°C, while the rest of the operations are the same.

[0072] The performance results of the tungsten-tantalum-nickel-iron-copper alloy obtained in Comparative Example 4 are shown in Table 1.

[0073] Comparative Example 5 The other conditions are the same as in Example 1, except that no heat treatment is performed after rotary forging. All other operations are the same.

[0074] The performance results of the tungsten-tantalum-nickel-iron-copper alloy obtained in Comparative Example 5 are shown in Table 1.

[0075] Comparative Example 6 The other conditions were the same as in Example 1. The difference from Example 1 was that stress-relief annealing was not performed after each stage of rotary forging (i.e., after each stage of rotary forging, the blank was not placed in a vacuum muffle furnace and held at 800°C for 10 minutes). Instead, the temperature was directly raised to 1000°C and held for 15 minutes before proceeding to the next stage of rotary forging. During the experiment, it was found that when the total deformation of rotary forging reached 15%, the sample cracked significantly and could not proceed to the next stage of rotary forging.

[0076] The performance results of the tungsten-tantalum-nickel-iron-copper alloys obtained in Examples 1-5 and Comparative Examples 1-5 are shown in Table 1.

[0077] Table 1 Performance test results of samples from Examples 1-5 and Comparative Examples 1-5 .

Claims

1. A method for preparing a high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties, characterized in that: The process includes rotary forging and heat treatment. The tungsten-tantalum-nickel-iron-copper alloy bars are first heated in a vacuum muffle furnace at 800~1300℃, and then placed in a rotary forging device for N-stage rotary forging. After rotary forging, the alloy is placed in a vacuum muffle furnace at 700~900℃ for high-temperature heat treatment for 5~10 hours, followed by furnace cooling. Then, it is subjected to low-temperature heat treatment at 400~500℃ for 1~5 hours, followed by furnace cooling to obtain the finished product. During the N-stage rotary forging process, the alloy after each stage of rotary forging is held in a vacuum muffle furnace at 700~900℃ for 5~30 minutes, then heated to 800~1300℃ and held for 10~30 minutes, and then the next stage of rotary forging is carried out. The deformation amount in each stage of rotary forging is 1~4.5%, and the total deformation amount in rotary forging is 20~70%; The tungsten-tantalum-nickel-iron-copper alloy is composed of (tungsten + tantalum), nickel, iron, and copper in a mass ratio of (tungsten + tantalum):nickel:iron:copper = 90:3.5~6.3:1.5~2.7:1~5; wherein the mass ratio of tungsten to tantalum is 85~95:5~15. The swaging process is as follows: the tungsten-tantalum-nickel-iron-copper alloy rod is placed in a vacuum muffle furnace for high-temperature heating, the vacuum degree is ≤1×10 -3 Pa, the heating rate is set to 15-35 ℃ / min, the temperature is 800-1300 ℃, and the temperature is kept for 10-30 min; then it is placed in a swaging equipment, and the swaging frequency is set to 1200 times / min.

2. The method for preparing a high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties according to claim 1, characterized in that: The tungsten-tantalum-nickel-iron-copper alloy rods are placed in a vacuum muffle furnace and heated at a high temperature of 900~1150℃.

3. The method for preparing a high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties according to claim 2, characterized in that: The tungsten-tantalum-nickel-iron-copper alloy rods are placed in a vacuum muffle furnace and heated at a high temperature of 950~1100℃.

4. The method for preparing a high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties according to claim 3, characterized in that: The tungsten-tantalum-nickel-iron-copper alloy rods were placed in a vacuum muffle furnace and heated at a high temperature of 980~1020℃.

5. The method for preparing a high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties according to claim 1, characterized in that: The deformation amount of each stage of rotary forging is 1.5~3.5%.

6. The method for preparing a high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties according to claim 1, characterized in that: The deformation amount in each stage of rotary forging is 1.5~3%.

7. The method for preparing a high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties according to claim 1, characterized in that: The deformation amount of each stage of rotary forging is 1.8~2.2%.

8. The method for preparing a high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties according to claim 1, characterized in that: The total deformation of rotary forging is 30-55%.

9. The method for preparing a high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties according to claim 1, characterized in that: The total deformation of rotary forging is 30-50%.

10. The method for preparing a high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties according to claim 1, characterized in that: The total deformation of rotary forging is 38-42%.

11. The method for preparing a high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties according to claim 1, characterized in that: Before each rotary forging, the high-temperature heating holding time is 10~30 minutes.

12. An application of a high-strength tungsten-tantalum-nickel-iron-copper alloy with self-sharpening properties as described in claim 1, characterized in that: The self-sharpening high-strength tungsten-tantalum-nickel-iron-copper alloy is used in armor-piercing projectile materials.

Citation Information

Patent Citations

  • A high-strength, ultrafine-grained tungsten-tantalum-nickel-iron-copper alloy, its preparation method, and its applications.

    CN115341112B

  • A heat treatment method for a tungsten-tantalum-nickel-iron-copper alloy

    CN117403158B

  • Heat treatment method of tungsten-tantalum-nickel-iron-copper alloy