Efficient crushing, grinding and dressing process for complex copper-nickel sulfide ore

By using high-pressure roller mills and hydrocyclones in the beneficiation process of copper-nickel sulfide ore, the grinding process was optimized, solving the problems of frequent grinding media replacement, high energy consumption, and difficulty in recovering precious metals. This achieved low energy consumption, low steel consumption, and high-efficiency grinding and classification, improving production efficiency and precious metal recovery rate.

CN118218116BActive Publication Date: 2026-11-24JINCHUAN GROUP NICKEL COBALT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410349893.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-26
Publication Date
2026-11-24
Estimated Expiration
2044-03-26

AI Technical Summary

Technical Problem

Existing copper-nickel sulfide ore beneficiation processes suffer from problems such as frequent grinding media replacement, high energy and steel consumption, low grinding and classification efficiency, and difficulty in effectively recovering associated precious metals.

Method used

High-pressure roller mills are used to replace cone crushers and rod mills, and combined with hydrocyclones and Nelson gravity separators to optimize the grinding and flotation process and achieve efficient crushing and beneficiation.

Benefits of technology

It reduced energy and steel consumption in production, improved the operating efficiency of the production system, increased the recovery rate of precious metals, and boosted the revenue of the beneficiation plant.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118218116B_ABST
    Figure CN118218116B_ABST
Patent Text Reader

Abstract

This invention discloses a high-efficiency crushing and beneficiation process for complex disseminated copper-nickel sulfide ores. Addressing the shortcomings of existing copper-nickel sulfide ore production processes, such as low operating rates of crushing and beneficiation systems, high energy and steel consumption, high production costs, low grinding and classification efficiency, and ineffective recovery of associated precious metals, this invention provides a high-efficiency crushing and beneficiation process for complex disseminated copper-nickel sulfide ores using high-pressure roller mills. This process is characterized by low energy consumption, low steel consumption, low production costs, high grinding and classification efficiency, and effective recovery of associated precious metals while simultaneously recovering copper-nickel sulfide ore. This invention completely replaces two short-head cone crushers and one rod mill with a single high-pressure roller mill, shortening the crushing and grinding process, reducing the number of operating equipment, extending the continuous beneficiation production time, and improving production efficiency. Energy consumption per unit product is reduced by more than 40%, steel consumption by more than 50%, and the annual operating rate of the production system is increased by more than 15%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the beneficiation process of nickel-copper sulfide ores, specifically to a high-efficiency crushing and grinding beneficiation process for complex interspersed copper-nickel sulfide ores. Background Technology

[0002] With the development and utilization of mineral resources, copper-nickel sulfide ores are gradually becoming "poor, fine-grained, and complex." The copper-nickel sulfide ores involved in this invention have nickel primarily occurring as nickel sulfide in pyrrhotite and sulphite, with over 80% of the nickel present in sulfides. Small amounts are also present in pyrrhotite and pyrite, and 15% of the nickel exists in oxide form. Furthermore, 27% of the nickel in pyrrhotite is smaller than 45 μm, and 24% in sulphite.

[0003] Copper is mainly found in chalcopyrite and chalcopyrite as sulfides, with a small amount found in pyrrhotite and pyrite. Copper accounts for up to 80% of the sulfide content, while copper minerals account for 16% of the gangue. Furthermore, analysis of the distribution characteristics of copper minerals in the gangue reveals that these minerals are encased in extremely fine gangue minerals, making them difficult to dissociate and recover, thus easily resulting in the loss of copper minerals.

[0004] This complex, disseminated copper-nickel sulfide ore currently employs a crushing and beneficiation process consisting of "cone crushing and screening + rod milling + two-stage ball milling and classification + two-stage flotation." After the ore is mined underground, it undergoes primary crushing in a gyratory crusher before being transported to the beneficiation plant. This product, as the raw ore, is then further crushed in a standard cone crusher. The product is then screened, and qualified particles are conveyed by belt conveyor to a powder silo for temporary storage as grinding feed. Unqualified particles are further crushed in a short-head cone crusher and screened, forming a closed-circuit screening process. Qualified particles from the powder silo are fed into a rod mill. After liberation, the product undergoes primary classification in the rod mill. The overflow is conveyed to a secondary pump tank in the first stage, and the underflow is conveyed to a primary ball mill for regrinding. The ball mill product undergoes primary classification in the first stage, forming a closed-circuit grinding process. The first stage of flotation involves two stages of grinding. The first stage of flotation uses a roughing and cleaning process to obtain a copper-nickel mixed concentrate with relatively high nickel and copper grades. The tailings from the first roughing and cleaning processes are fed into a second-stage ball mill for grinding. The ground product undergoes secondary classification in the second stage, and the overflow enters the second-stage flotation process. The tailings are returned to the second-stage ball mill for further liberation, forming a second-stage closed-circuit grinding process. The second stage of flotation uses a roughing, cleaning, and scavenging process to obtain a copper-nickel mixed concentrate and tailings with relatively low nickel and copper grades. The tailings from the first cleaning and scavenging processes are returned to the second-stage pump tank for second-stage closed-circuit grinding and classification.

[0005] The shortcomings of this method are: (1) The grinding media of the rod mill needs to be replaced every 15 days, which affects the overall operating efficiency of the beneficiation plant; (2) The power consumption of the rod mill and ball mill is high, consuming more than 20 kWh of electricity per ton of ore, accounting for more than 70% of the total power consumption of the plant; (3) The steel consumption of the rod mill and ball mill is high, requiring 1.5 kg of steel balls and liners per ton of ore, accounting for more than 85% of the total steel consumption of the plant; (4) Nickel, copper and their associated platinum and gold minerals are hard, and the existing "cone + rod mill + ball mill" crushing and grinding process has over-grinding phenomenon. The proportion of nickel, copper and their associated platinum and gold minerals below -10μm is 10%-15%, which cannot be effectively recovered by flotation. The platinum and gold grades in copper-nickel mixed gold ore are low and cannot reach the pricing coefficient, thus failing to improve the revenue of the beneficiation plant.

[0006] The invention patent (authorization number: CN 102179284 B) "Method for Crushing Iron Ore" uses a "closed-circuit process of high-pressure roller milling and screening" to reduce the particle size of the raw material entering the mill, thereby reducing the grinding Bond work index. This process is only applicable to magnetite ore. If the copper-nickel sulfide ore has a complex mineral distribution and is associated with high-value platinum, gold, etc., the copper-nickel sulfide minerals and their associated precious metal minerals cannot be recovered in one flotation step, resulting in the copper-nickel sulfide ore and their associated precious metal minerals entering the tailings and causing a large loss. Summary of the Invention

[0007] The purpose of this invention is to address the shortcomings of existing copper-nickel sulfide ore production processes, such as low operating rates of grinding and beneficiation systems, high energy and steel consumption, high production costs, low grinding and classification efficiency, and ineffective recovery of associated precious metals. This invention provides a high-efficiency grinding and beneficiation process for complexly embedded copper-nickel sulfide ore using high-pressure roller mills, which features low energy consumption, low steel consumption, low production costs, high grinding and classification efficiency, and effective recovery of associated precious metals while simultaneously recovering copper-nickel sulfide ore.

[0008] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A high-efficiency crushing and beneficiation process for complex disseminated copper-nickel sulfide ores includes the following steps: (1) The complex interspersed copper-nickel sulfide ore is transported to a standard cone crusher for coarse crushing; (2) The product after coarse crushing in step (1) is transported to the high-pressure roller mill for fine crushing. After fine crushing, the central material is directly transported to the powder ore bin for storage, and the edge material on both sides is transported to the vibrating screen for screening. The unqualified products are returned to the high-pressure roller mill for secondary fine crushing. The qualified products are transported to the powder ore bin for storage, and then transported to the ball mill by the feeder and belt conveyor for subsequent processing. (3) The product stored in the powder ore bin in step (2) is transported to the first-stage ball mill for grinding. After the product is diluted with water and slurry is prepared, it enters the first-stage pump pool. The slurry is pumped through the pipeline to the first-stage hydrocyclone for first-stage pre-classification. The overflow product flows by gravity through the pipeline to the first-stage secondary pump pool. The sand product is returned to the first-stage ball mill for further separation, forming a first-stage closed-circuit grinding.

[0009] (4) The overflow product from the first stage of primary classification that enters the secondary pump pool in step (3) is transported by slurry pump through pipeline to the secondary hydrocyclone of the first stage for inspection and classification. The overflow product flows by gravity through pipeline to the stirring tank of the first stage flotation process. The sand product is mixed with water and then enters the stirring tank. It flows by gravity through pipeline to the Nelson gravity separator to enrich the platinum and gold precious metals associated in the ore, producing precious metal concentrate. The tailings enriched by the Nelson gravity separator flow by gravity through pipeline to the secondary ball mill of the first stage for dissociation. The product is diluted with water and then enters the secondary pump pool of the first stage. It is transported by slurry pump through pipeline to the secondary hydrocyclone of the first stage for inspection and classification, forming a secondary closed-circuit grinding process.

[0010] (5) Add water to the first secondary grade overflow product obtained in step (4) to adjust the slurry, add collector, frother and dispersant to mineralize the copper-nickel mixed ore, and then carry out first primary roughing, first primary cleaning and first secondary cleaning to obtain high-grade copper-nickel mixed concentrate.

[0011] (6) The tailings from the first roughing and first cleaning in step (5) are fed by gravity through a pipeline to the second ball mill for second-stage grinding and dissociation. The product is mixed with water and then enters the second pump pool. The slurry is pumped by a slurry pump through a pipeline to the second hydrocyclone for classification. The overflow product is fed by gravity through a pipeline to the second flotation mixing tank. The sand product is returned to the second ball mill for further grinding, forming a closed-loop cycle of second-stage grinding.

[0012] (7) Add water to the two-stage graded overflow product obtained in step (6) to adjust the slurry, add collector, frother and dispersant to remineralize the copper-nickel mixed ore, and then carry out two-stage first roughing, two-stage first cleaning, two-stage second cleaning, two-stage first scavenging and two-stage second scavenging to obtain low-grade copper-nickel mixed concentrate and final tailings.

[0013] In step (1), a standard cone crusher is used for coarse crushing, and the discharge opening is controlled at 50-20mm.

[0014] In step (2), the vibrating screen is a dry linear vibrating screen and the screen mesh is a 12mm×32mm strip screen.

[0015] In step (3), the ball mill is an overflow ball mill, the grinding media is high chromium balls, the model is Φ80mm and Φ90mm, and the mass ratio is 1:1; the first stage hydrocyclone is a volute pre-classification large cone angle hydrocyclone.

[0016] In step (4), the first-stage secondary hydrocyclone adopts a volute pre-classification long conical hydrocyclone. The grinding media of the first-stage secondary ball mill is made of cast iron, with a model of 40mm×45mm. After the sand product from the first-stage secondary hydrocyclone is diluted with water to a slurry with an ore mass percentage of 40%-45%, the precious metals in the ore are enriched by a Nelson gravity separator to obtain a precious metal concentrate with a Pt grade of 180-450g / t and an Au grade of 30-180g / t.

[0017] In step (5), the overflow product from the first-stage secondary hydrocyclone has a fineness of -200 mesh and a mass percentage of 65%-72%. The first-stage secondary overflow product is diluted with water to a slurry with a ore mass percentage of 25%-35%. The dosage of collector is 160-220 g / t, frother is 40-75 g / t, and dispersant is 80-300 g / t. Through one roughing and two cleaning processes, a high-grade copper-nickel mixed concentrate with a nickel grade of 6%-12% and a copper grade of 4%-9% is obtained.

[0018] In step (6), the fineness of the overflow product from the second-stage hydrocyclone is controlled to be 80%-88% by mass of -200 mesh. The overflow product from the second stage is diluted with water to a slurry with a ore mass percentage of 18%-30%.

[0019] In step (7), the amount of collector added is 40-80 g / t, the amount of frother added is 0-40 g / t, and the amount of dispersant added is 0-200 g / t. Through one roughing, two cleaning, and two scavenging processes, a low-grade copper-nickel mixed concentrate with a nickel grade of 3.8%-5.5% and a copper grade of 1.5%-3.5% and the final tailings containing 0.15%-0.22% nickel and 0.10%-0.25% copper are obtained.

[0020] In step (7), the tailings from the first stage of secondary beneficiation and the concentrate from the first stage of secondary scavenging are returned to the secondary pump pool and subjected to secondary closed-circuit grinding and classification with the product from the secondary ball mill in step (6).

[0021] The beneficial effects of this invention are as follows: High-pressure roller mills, as crushing and grinding equipment, are only used for ultrafine crushing of ore or, to improve system processing capacity, are used in conjunction with cone crushers for further crushing of ore during the crushing stage. In this invention, the high-pressure roller mill not only replaces the short-head cone crusher (which has a relatively low crushing ratio and efficiency) in the crushing stage, but also replaces the high-energy-consuming and high-steel-consuming rod mill in the grinding stage, shortening the crushing and grinding process and reducing the number of equipment requiring operation and maintenance. Furthermore, the production system does not need to be shut down entirely due to replacing or adding grinding media to the rod mill, thus increasing the production system's operating time and improving its operational efficiency. This invention's method completely replaces two short-head cone crushers and one rod mill with one high-pressure roller mill, shortening the crushing and grinding process, reducing the number of operating equipment, extending the continuous beneficiation production operating time, and improving production efficiency. Energy consumption per unit product is reduced by more than 40%, steel consumption by more than 50%, and the annual operating rate of the production system is increased by more than 15%.

[0022] Meanwhile, the high-pressure roller mill's high crushing efficiency reduces the ball mill's Bond work index and separates rare and precious metals such as platinum and gold associated with copper-nickel sulfide ores from the complexly embedded ore, improving grinding and classification efficiency and effectively recovering associated precious metals. The classification efficiency of the first stage has increased by more than 15%, and the beneficiation plant has added a precious metal concentrate product, increasing revenue by 10%. Attached Figure Description

[0023] Figure 1 This is a flow chart of the grinding process of the present invention. Detailed Implementation

[0024] Example 1 like Figure 1 As shown, a high-efficiency crushing and grinding beneficiation process for complex disseminated copper-nickel sulfide ores includes the following steps: (1) The particle size content P 100 Complex copper-nickel sulfide ores with a diameter of ≤350mm are transported to a standard cone crusher for primary crushing, and the discharge port gap is adjusted to 38mm.

[0025] (2) The product from step (1) is fed to a high-pressure roller mill for fine crushing. The gap between the high-pressure roller mills is adjusted to 23 mm. The finely crushed core material product P 80 ≤12mm, are conveyed to the powder silo for storage, and the edge products on both sides are conveyed to the vibrating screen for screening. The screen hole size is controlled to be 12mm×28mm. Unqualified products are returned to the high-pressure roller mill for secondary crushing. Qualified products are conveyed to the powder silo for storage, and then conveyed to the ball mill by the feeder and belt conveyor for further processing. (3) The product stored in the powder silo in step (2) is transported to the primary ball mill for grinding. After the product is diluted with water and adjusted to a ore mass percentage of 40%, it enters the primary pump pool of the primary stage. The slurry is then pumped through the pipeline to the primary hydrocyclone of the primary stage for primary stage pre-classification. The fineness of the qualified overflow product is controlled to be -200 mesh, accounting for 50%. The product flows by gravity through the pipeline to the secondary pump pool of the primary stage. The sand product is returned to the primary ball mill of the primary stage for further separation, forming a closed-loop grinding process in the primary stage. The ball mill is an overflow type ball mill. The grinding media material is high-chromium balls, with models of Φ80mm and Φ90mm, and the addition ratio is 1:1. The primary hydrocyclone of the primary stage is a volute pre-classification large cone angle hydrocyclone.

[0026] (4) The qualified overflow product from the first stage of primary classification that entered the secondary pump tank in step (3) is transported by slurry pump through pipeline to the secondary hydrocyclone of the first stage for inspection and classification. The fineness of the qualified overflow product is controlled to be -200 mesh, accounting for 68%. It is then transported to the stirring tank of the first stage flotation process. The sand product is mixed with water to adjust the ore mass percentage to 40% and then enters the stirring tank. It flows by gravity through pipeline to the Nelson gravity separator to enrich the associated precious metals such as platinum and gold in the ore, obtaining a precious metal concentrate with a Pt grade of 400 g / t and an Au grade of 180 g / t. The tailings enriched by the Nelson gravity separator flow by gravity through pipeline to the secondary ball mill of the first stage for dissociation. The product is diluted with water and then enters the secondary pump tank of the first stage. It is then transported by slurry pump through pipeline to the secondary hydrocyclone of the first stage for inspection and classification, forming a secondary closed-circuit grinding process. The secondary hydrocyclone of the first stage adopts a volute pre-classification long cone hydrocyclone. The grinding media of the first-stage secondary ball mill are made of cast iron, with a size of 40mm×45mm.

[0027] (5) Dilute the first secondary grade overflow product obtained in step (4) with water to a slurry with an ore mass percentage of 35%, add collector (sodium isobutyl xanthate) 180g / t, frother (BQ-622) 70g / t, dispersant (sodium hexametaphosphate) 250g / t, mineralize the copper-nickel sulfide ore containing 1.4% nickel and 1.1% copper, and then carry out a first primary roughing, a first primary cleaning and a first secondary cleaning to obtain a high-grade copper-nickel mixed concentrate with a nickel grade of 11.8% and a copper grade of 8.9%.

[0028] (6) The tailings from the first roughing and first cleaning in step (5) are transported to the second ball mill for grinding via pipeline. The product is diluted with water to a slurry with a ore mass percentage of 30%, and then transported to the second hydrocyclone for classification via pipeline by a slurry pump. The fineness of the qualified overflow product is controlled to be -200 mesh, accounting for 85%, and then transported to the second flotation mixing tank. The sand product is returned to the second ball mill for further grinding, forming a closed-loop cycle of second-stage grinding.

[0029] (7) Dilute the two-stage graded overflow product obtained in step (6) with water to 23% of the ore mass. Add 80g / t of collector (sodium isobutyl xanthate), 40g / t of frother (BQ-622), and 200g / t of dispersant (sodium hexametaphosphate) to remineralize the copper-nickel mixed ore. Then, perform one roughing, two cleaning, and two scavenging to obtain a low-grade copper-nickel mixed concentrate with a nickel grade of 5.0% and a copper grade of 3.5% and a final tailings containing 0.22% nickel and 0.25% copper.

[0030] Example 2 like Figure 1 As shown, a high-efficiency crushing and grinding beneficiation process for complex disseminated copper-nickel sulfide ores includes the following steps: (1) The particle size content P 100 Complex copper-nickel sulfide ores with a diameter of ≤350mm are transported to a standard cone crusher for primary crushing, and the discharge port gap is adjusted to 42mm.

[0031] (2) The product from step (1) is fed to a high-pressure roller mill for fine crushing. The gap between the high-pressure roller mills is adjusted to 23 mm. The core material product P after crushing is... 80 ≤12mm, are conveyed to the powder silo for storage, and the edge products on both sides are conveyed to the vibrating screen for screening. The screen hole size is controlled to be 12mm×32mm. Unqualified products are returned to the high-pressure roller mill for secondary crushing. Qualified products are conveyed to the powder silo for storage, and then conveyed to the ball mill by the feeder and belt conveyor for further processing. (3) The product stored in the powder silo in step (2) is transported to the first-stage ball mill for grinding. The product is diluted with water and adjusted to a ore mass percentage of 40% before being pre-classified in the first stage. The fineness of the qualified overflow product is controlled to be -200 mesh, accounting for 50%. The product flows by gravity through the pipeline to the second-stage pump pool in the first stage. The sand product is returned to the first-stage ball mill in the first stage for further separation, forming a closed-circuit grinding in the first stage.

[0032] (4) The qualified overflow product from the first stage of classification in step (3) is transported to the second stage of inspection and classification. The fineness of the qualified overflow product is controlled to be 65% -200 mesh. It is then transported to the first stage flotation process mixing tank. The sand product is mixed with water to adjust the ore mass percentage to 42% and then enters the mixing tank. It flows by gravity through the pipeline to the Nelson gravity separator to enrich the associated precious metals such as platinum and gold in the ore, and obtains a precious metal concentrate with a Pt grade of 220 g / t and an Au grade of 100 g / t. The tailings enriched by the Nelson gravity separator flow by gravity through the pipeline to the first stage secondary ball mill for dissociation. The product is diluted with water and then enters the first stage secondary pump pool. It is then transported by the slurry pump through the pipeline to the first stage secondary hydrocyclone for inspection and classification, forming a first stage secondary closed-circuit grinding.

[0033] (5) Dilute the secondary grade overflow product obtained in step (4) with water to a slurry with an ore mass percentage of 30%, add collector (sodium ethyl xanthate) 160g / t, frother (butyl ammonium black powder) 60g / t, dispersant (ammonium sulfate) 80g / t, mineralize the copper-nickel sulfide ore containing 0.78% nickel and 0.52% copper, and then perform a roughing and a cleaning process to obtain a high-grade copper-nickel mixed concentrate with a nickel grade of 6.5% and a copper grade of 4.2%.

[0034] (6) The tailings from the first roughing and first cleaning in step (5) are transported to the second ball mill for grinding via pipeline. The product is diluted with water to a slurry with a ore mass percentage of 35% and then classified. The fineness of the qualified overflow product is controlled to be -200 mesh, accounting for 88%. The product is then transported to the second flotation mixing tank. The sand product is returned to the second ball mill for further grinding, forming a closed-loop cycle of the second grinding.

[0035] (7) Dilute the two-stage graded overflow product obtained in step (6) with water to 20% of the ore mass. Add 60g / t of collector (sodium ethyl xanthate), 0g / t of frother and 0g / t of dispersant to remineralize the copper-nickel mixed ore. Then, perform one roughing, two cleaning and two scavenging to obtain a low-grade copper-nickel mixed concentrate with a nickel grade of 4.0% and a copper grade of 2.3% and a final tailings with a nickel grade of 0.17% and a copper grade of 0.10%.

[0036] Example 3 like Figure 1 As shown, a high-efficiency crushing and grinding beneficiation process for complex disseminated copper-nickel sulfide ores includes the following steps: (1) The particle size content P 100 Complex copper-nickel sulfide ores with a diameter of ≤300mm are transported to a standard cone crusher for primary crushing, and the discharge port gap is adjusted to 50mm.

[0037] (2) The product from step (1) is fed to a high-pressure roller mill for fine crushing. The gap between the high-pressure roller mills is adjusted to 26 mm. The core material P after crushing 80 ≤12mm, are conveyed to the powder silo for storage, and the edge products on both sides are conveyed to the vibrating screen for screening. The screen hole size is controlled to be 12mm×25mm. Unqualified products are returned to the high-pressure roller mill for secondary crushing. Qualified products are conveyed to the powder silo for storage, and then conveyed to the ball mill by the feeder and belt conveyor for further processing. (3) The product stored in the powder silo in step (2) is transported to the first-stage ball mill for grinding. The product is diluted with water and adjusted to a ore mass percentage of 40% before being pre-classified in the first stage. The fineness of the qualified overflow product is controlled to be -200 mesh, accounting for 50%. The product flows by gravity through the pipeline to the second-stage pump pool in the first stage. The sand product is returned to the first-stage ball mill in the first stage for further separation, forming a closed-circuit grinding in the first stage.

[0038] (4) The qualified overflow product from the first stage of classification in step (3) is transported to the second stage of inspection and classification. The fineness of the qualified overflow product is controlled to be 70% -200 mesh. It is then transported to the first stage flotation process mixing tank. The sand product is mixed with water to adjust the ore mass percentage to 45% and then enters the mixing tank. It flows by gravity through the pipeline to the Nelson gravity separator to enrich the associated precious metals such as platinum and gold in the ore, and obtains precious metal concentrate with Pt grade of 180 g / t and Au grade of 40 g / t. The tailings enriched by the Nelson gravity separator flow by gravity through the pipeline to the first stage secondary ball mill for dissociation. The product is diluted with water and then enters the first stage secondary pump pool. It is then transported by the slurry pump through the pipeline to the first stage secondary hydrocyclone for inspection and classification, forming the first stage secondary closed-circuit grinding.

[0039] (5) Dilute the secondary grade overflow product obtained in step (4) with water to a slurry with an ore mass percentage of 32%, add collector (sodium ethyl xanthate) 140g / t, frother (butyl ammonium black powder) 60g / t and dispersant 0g / t, mineralize the copper-nickel sulfide ore containing 0.52% nickel and 0.38% copper, and then perform a roughing and a cleaning process to obtain a high-grade copper-nickel mixed concentrate with a nickel grade of 6.0% and a copper grade of 3.2%.

[0040] (6) The tailings from the first roughing and first cleaning in step (5) are transported to the second ball mill for grinding via pipeline. The product is diluted with water to a slurry with a ore mass percentage of 35% and then classified. The fineness of the qualified overflow product is controlled to be -200 mesh, accounting for 85%. The product is then transported to the second flotation mixing tank. The sand product is returned to the second ball mill for further grinding, forming a closed-loop cycle of the second grinding.

[0041] (7) Dilute the two-stage graded overflow product obtained in step (6) with water to 17% of the ore mass. Add 40g / t of collector (sodium ethyl xanthate), 0g / t of frother and 0g / t of dispersant to remineralize the copper-nickel mixed ore. Then, perform one roughing, two cleaning and two scavenging to obtain a low-grade copper-nickel mixed concentrate with a nickel grade of 4.0% and a copper grade of 2.2% and a final tailings containing 0.15% nickel and 0.10% copper.

Claims

1. A high-efficiency crushing and grinding beneficiation process for complex disseminated copper-nickel sulfide ores, comprising the following steps: (1) The complex interspersed copper-nickel sulfide ore is transported to a standard cone crusher for coarse crushing; (2) The product after coarse crushing in step (1) is transported to the high-pressure roller mill for fine crushing. After fine crushing, the central material is directly transported to the powder ore bin for storage, and the edge material on both sides is transported to the vibrating screen for screening. The unqualified products are returned to the high-pressure roller mill for secondary fine crushing. The qualified products are transported to the powder ore bin for storage, and then transported to the ball mill by the feeder and belt conveyor for subsequent processing. (3) The product stored in the powder ore bin in step (2) is transported to the first-stage ball mill for grinding. After the product is diluted with water and slurry is prepared, it enters the first-stage pump pool. The slurry is pumped through the pipeline to the first-stage hydrocyclone for first-stage pre-classification. The overflow product flows by gravity through the pipeline to the first-stage secondary pump pool. The sand product is returned to the first-stage ball mill for further separation, forming a first-stage closed-circuit grinding. (4) The overflow product from the primary classification in step (3) is pumped by a slurry pump through a pipeline to the secondary hydrocyclone for inspection and classification. The overflow product flows by gravity through a pipeline to the flotation process mixing tank. The sand product is mixed with water and then enters the mixing tank. It flows by gravity through a pipeline to the Nelson gravity separator to enrich the associated platinum and gold precious metals in the ore, producing precious metal concentrate. The tailings enriched by the Nelson gravity separator flow by gravity through a pipeline to the secondary ball mill for dissociation. The product is diluted with water and then enters the secondary pump pool. It is pumped by a slurry pump through a pipeline to the secondary hydrocyclone for inspection and classification, forming a secondary closed-circuit grinding process. (5) Add water to the overflow product obtained in step (4) to adjust the slurry, add collector, frother and dispersant to mineralize the copper-nickel mixed ore, and then carry out a first-stage roughing, a first-stage cleaning and a second-stage cleaning to obtain high-grade copper-nickel mixed concentrate. (6) The tailings from the first roughing and first cleaning in step (5) are fed by gravity through a pipeline to the second ball mill for second-stage grinding and dissociation. The product is mixed with water and then enters the second pump pool. The slurry is pumped by a slurry pump through a pipeline to the second hydrocyclone for classification. The overflow product is fed by gravity through a pipeline to the second flotation mixing tank. The sand product is returned to the second ball mill for further grinding, forming a closed-loop cycle of second-stage grinding. (7) Add water to the two-stage graded overflow product obtained in step (6) to adjust the slurry, add collector, frother and dispersant to remineralize the copper-nickel mixed ore, and then carry out two-stage first roughing, two-stage first cleaning, two-stage second cleaning, two-stage first scavenging and two-stage second scavenging to obtain low-grade copper-nickel mixed concentrate and final tailings.

2. The efficient crushing and grinding beneficiation process for complex embedded copper-nickel sulfide ores according to claim 1, characterized in that: In step (1), a standard cone crusher is used for coarse crushing, and the discharge opening is controlled at 50-20mm.

3. The efficient crushing and grinding beneficiation process for complex embedded copper-nickel sulfide ores according to claim 1, characterized in that: In step (2), the vibrating screen is a dry linear vibrating screen and the screen mesh is a 12mm×32mm strip screen.

4. The efficient crushing and grinding beneficiation process for complex embedded copper-nickel sulfide ores according to claim 1, characterized in that: In step (3), the ball mill is an overflow ball mill, the grinding media is high chromium balls, the model is Φ80mm and Φ90mm, and the mass ratio is 1:1; the first stage hydrocyclone is a volute pre-classification large cone angle hydrocyclone.

5. The efficient crushing and grinding beneficiation process for complex embedded copper-nickel sulfide ores according to claim 1, characterized in that: In step (4), the first-stage secondary hydrocyclone adopts a volute pre-classification long cone hydrocyclone; the grinding media of the first-stage secondary ball mill is made of cast iron with a model of 40mm×45mm; after the sand product of the first-stage secondary hydrocyclone is diluted with water to a slurry with an ore mass percentage of 40%-45%, the precious metals in the ore are enriched by a Nelson gravity separator to obtain a precious metal concentrate with a Pt grade of 180-450g / t and an Au grade of 30-180g / t.

6. The efficient crushing and grinding beneficiation process for complex embedded copper-nickel sulfide ores according to claim 1, characterized in that: In step (5), the overflow product of the first-stage secondary hydrocyclone has a fineness of -200 mesh and a mass percentage of 65%-72%; the overflow product of the first-stage secondary hydrocyclone is diluted with water to a slurry with a ore mass percentage of 25%-35%; the amount of collector added is 160-220g / t, the amount of frother is 40-75g / t, and the amount of dispersant is 80-300g / t; through one roughing and two cleaning processes, a high-grade copper-nickel mixed concentrate with a nickel grade of 6%-12% and a copper grade of 4%-9% is obtained.

7. The efficient crushing and grinding beneficiation process for complex embedded copper-nickel sulfide ores according to claim 1, characterized in that: In step (6), the fineness of the overflow product from the second-stage hydrocyclone is controlled to be -200 mesh with a mass percentage of 80%-88%; the overflow product from the second stage is diluted with water to a slurry with a ore mass percentage of 18%-30%.

8. The efficient crushing and grinding beneficiation process for complex embedded copper-nickel sulfide ores according to claim 1, characterized in that: In step (7), the amount of collector added is 40-80 g / t, the amount of frother added is 0-40 g / t, and the amount of dispersant added is 0-200 g / t. Through one roughing, two cleaning, and two scavenging processes, a low-grade copper-nickel mixed concentrate with a nickel grade of 3.8%-5.5% and a copper grade of 1.5%-3.5% and the final tailings containing 0.15%-0.22% nickel and 0.10%-0.25% copper are obtained.

9. The efficient crushing and grinding beneficiation process for complex embedded copper-nickel sulfide ores according to claim 1, characterized in that: In step (7), the tailings from the first stage of secondary beneficiation and the concentrate from the first stage of secondary scavenging are returned to the secondary pump pool and subjected to secondary closed-circuit grinding and classification with the product from the secondary ball mill in step (6).

Citation Information

Patent Citations

  • Method for crushing iron ore

    CN102179284B

  • Low-grade mineral separation process

    CN113731625A

  • Efficient crushing and grinding equipment for fine-particle embedded copper-nickel ore

    CN216856974U