A beneficiation process for recovering precious metals in a copper-nickel sulfide ore whole process
By optimizing the entire beneficiation process of copper-nickel sulfide ore, and combining steps such as grinding, flotation, desliming and magnetic separation, the problem of low recovery rate of associated precious metals in copper-nickel sulfide ore has been solved, achieving efficient recovery and resource utilization, reducing the loss of precious metals in tailings, and improving economic benefits and environmental safety.
Patent Information
- Application Number
- CN202410349907.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-26
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-03-26
AI Technical Summary
In existing technologies, the recovery rate of associated precious metals in copper-nickel sulfide ores is low, the process is complex, and the tailings are difficult to handle, resulting in resource waste and environmental pollution. Existing Nelson concentrators frequently malfunction, affecting production.
A mineral processing technology for the complete recovery of precious metals from copper-nickel sulfide ores is adopted, which includes primary grinding, classification and Nelson gravity separation, combined with flotation, desliming, magnetic separation and felt beneficiation steps, and optimizes reagent use and equipment parameters to achieve efficient recovery of precious metals.
It improves the overall recovery rate of precious metals, reduces the loss of precious metals in tailings, enhances economic benefits and resource utilization, solves the problem of tailings treatment, and avoids environmental pollution.
Smart Images

Figure CN118218117B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of non-ferrous metal mineral beneficiation technology, specifically relating to a beneficiation process for the complete recovery of precious metals from copper-nickel sulfide ores. Background Technology
[0002] The Nelson concentrator is an enhanced gravity separation device based on the centrifugal principle. In an enhanced gravity field, the separation between light and heavy minerals is easier than in a natural gravity field; this equipment has become the preferred gravity separation equipment in non-ferrous metal beneficiation plants where precious metals are associated with other minerals. Existing intermittent discharge Nelson concentrators require shutdown to discharge concentrate every 1-2 hours. Furthermore, Nelson concentrators frequently experience malfunctions due to issues such as the enrichment cone, affecting the production of precious metal concentrates and the recovery of nickel and copper metals in the main process.
[0003] Mining enterprises generally face the problem of difficult tailings disposal, resulting in low comprehensive utilization rates and serious waste of tailings resources, while also jeopardizing the surrounding environment. Associated precious metals, including rare and precious metals such as gold, silver, platinum, and palladium, are difficult to recover effectively. Methods for recovering precious metals from gravity-separated tailings mainly employ processes such as Nelson gravity separation and a combination of gravity separation and flotation. Given the dwindling mineral resources, secondary recovery of precious metals from tailings is a worthy area of research. This can not only improve the recovery rate and utilization rate of precious metals in tailings but also enhance the economic benefits of metallurgical enterprises.
[0004] Precious metals are often associated with nickel-copper sulfide ores in China. To broaden the channels for precious metal resources and the utilization scope of these associated precious metals, it is crucial to develop these resources and avoid their disposal in tailings. Therefore, developing new mineral processing technologies to rationally and efficiently recover associated precious metals like gold has become an urgent issue.
[0005] The main problems in recovering associated metals from copper-nickel sulfide ores are as follows: Chinese invention patent "A mineral processing method for recovering polymetals from gold-bearing gravity separation tailings", patent number CN112657670 B, discloses a mineral processing method for recovering polymetals from gold-bearing gravity separation tailings. Its process is complex and does not consider the recovery of precious metals from the entire mineral processing process. Summary of the Invention
[0006] This invention addresses the problems of complex processes and low recovery rates in existing copper-nickel sulfide ore recovery processes by providing an economical, efficient, and energy-saving beneficiation process that enables the complete recovery of precious metals from copper-nickel sulfide ore, ultimately improving the overall recovery rate of precious metals.
[0007] Therefore, the present invention adopts the following technical solution: A mineral processing technology for the complete recovery of precious metals from copper-nickel sulfide ores includes the following steps: 1) After the nickel-copper ore is ground once, it is then subjected to primary classification, secondary classification and Nilsson gravity separation 1 operation in sequence; The middlings from the first classification are returned to the first grinding stage, the middlings from the second classification enter the first roughing stage, and the middlings from Nelson gravity separation 1 undergo a third classification. The third-classification underflow is then combined with the third-classification overflow after a second grinding stage and returned to the second classification stage. The product of Nelson gravity separation 1 is precious metal concentrate 1. 2) After the first stage of roughing, a first stage of cleaning and felt beneficiation are carried out in sequence; The middlings from the roughing process and the middlings from the first beneficiation process enter the fourth grading stage. The products of felt beneficiation 1 are precious metal concentrate 2 and high-grade nickel-copper concentrate. 3) After four stages of overflow, two-stage roughing, two-stage cleaning, and felt beneficiation operations are carried out in sequence; Among them, the middlings from the fourth grade are returned to the fourth grade after two stages of grinding; the middlings from the second stage roughing are subjected to a second stage of scavenging; the middlings from the second stage cleaning are returned to the fourth grade; the products of felt beneficiation 2 are precious metal concentrate 3 and low-grade nickel-copper concentrate. 4) The tailings of the two-stage scavenging operation are subjected to three operations in sequence: primary desliming, secondary desliming, magnetic separation, sluice box beneficiation, and felt beneficiation. Among them, the middlings from the second-stage scavenging are returned to the fourth stage of classification. The tailings from the first desliming, second desliming, magnetic separation, sluice box beneficiation, and felt beneficiation 3 are combined into the total tailings. The product of felt beneficiation 3 is precious metal concentrate 4.
[0008] Further, in step 1), the nickel-copper ore particle size is -13mm, the primary grinding concentration is 60%, and the steel balls used in the primary grinding are 90mm, 80mm, and 60mm, respectively, in a weight ratio of 3:1:1; the secondary ball milling uses 50mm*60mm and 35mm*40mm cast iron segments in a weight ratio of 1:1.
[0009] Further, in step 2), the amount of butyl xanthate collector used in the roughing flotation reagent is 160g / t-180g / t of raw ore, the amount of ethyl xanthate used is 40g / t-80g / t of raw ore, the amount of ammonium sulfate used as modifier is 700g / t-800g / t of raw ore, and the amount of BQ-622 used as frother is 40-60g / t of raw ore.
[0010] Furthermore, in step 2), the content of the coarse particle size of -0.074mm is 65%-70%, and the gold panning cloth used in the felt beneficiation operation is 50cm*300cm, made of fiber, with a pile height of 13mm.
[0011] Further, in step 3), the content of -0.074mm particles in the second-stage roughing is 80%-85%, the amount of ethyl xanthate collector used in the second-stage roughing flotation is 80g / t-100g / t of raw ore, the amount of ammonium sulfate used as the modifier is 250g / t-300g / t of raw ore, and the amount of BQ-622 used as the frother is 10-20g / t of raw ore.
[0012] Furthermore, in step 4), the primary and secondary desliming processes use desliming hydrocyclones, with a feed concentration of 35%-40% and a feed pressure of 0.08-0.12 MPa. The magnetic separation equipment is a wet magnetic separator with a magnetic field strength of 1300 Gauss; For regrinding magnetic concentrate, ceramic balls are used as the grinding media. The ceramic balls are mixed with 25mm, 20mm and 15mm steel balls in a weight ratio of 2:1:1. The content of -0.074mm in the grinding product accounts for 81%-84% of the total particle size.
[0013] Furthermore, the felt beneficiation operation 1 uses 50cm*300cm gold panning cloth, made of fiber, with a pile height of 13mm. The felt beneficiation operation 2 uses 50cm*300cm long-pile gold panning straw, made of low-density polyethylene, with a pile height of 15cm. The felt beneficiation operation 3 uses 50cm*300cm long-pile gold panning straw, made of low-density polyethylene, with a pile height of 13cm.
[0014] The beneficial effects of this invention are as follows: 1. This invention proposes a process flow for recovering associated precious metals from nickel-copper sulfide ore through the entire process of grinding, flotation concentrate, and tailings. Without affecting the recovery of nickel and copper metals in the main process, it improves the recovery of associated precious metal resources, realizes the early recovery of precious metals during the grinding process, recovers a large amount of high-grade precious metals in the concentrate, and reduces the loss of precious metals in the tailings. 2. This invention proposes an innovative process for tailings desliming, followed by magnetic separation, and then sluice box beneficiation and felt enrichment of precious metals from the magnetic concentrate. This process reduces the loss of precious metals from tailings. It boasts advantages such as high economic efficiency and strong operability, improving the comprehensive utilization rate and added value of associated precious metal resources in nickel-copper ore, and has broad practical significance. Attached Figure Description
[0015] Figure 1 This is a process flow diagram of the mineral processing technology for the complete recovery of precious metals from copper-nickel sulfide ore according to the present invention. Figure 2 This is a schematic diagram of the traditional copper-nickel sulfide ore processing flow. Detailed Implementation
[0016] The present invention will be further described below with reference to specific embodiments: Example 1 In this embodiment, the raw ore contains 1.57% nickel and 1.34% copper. The nickel mainly exists in the form of nickel sulfide minerals, and the main gangue mineral is serpentine.
[0017] Mineral processing according to Figure 1 Steps to be performed: 1) After the -13mm raw ore undergoes a first-stage grinding process, it is successively subjected to a first-stage hydrocyclone classification, a second-stage hydrocyclone classification, and the Nelson gravity separation 1 operation. The middlings from the first-stage hydrocyclone classification are returned to the first-stage grinding process. The middlings from the second-stage hydrocyclone classification are slurries with a -0.074mm content of 68% and enter the first-stage roughing process. The middlings from the Nelson gravity separation 1 undergo a third-stage classification process. The underflow from the third-stage classification is then combined with the overflow from the third-stage classification and returned to the second-stage classification process. The product of the Nelson gravity separation 1 is precious metal concentrate 1.
[0018] 2) The middlings from the secondary classification consist of a slurry with a -0.074mm content of 68%. Reagents are added per ton of raw ore: 170g butyl xanthate, 60g ethyl xanthate, 800g ammonium sulfate, and 50g BQ-622. A roughing operation is then performed. The flotation product, without reagent addition, proceeds to a cleaning operation. The cleaning product is then subjected to felt beneficiation 1, using 13mm thick fiber gold panning cloth. The middlings from the primary roughing and cleaning operations are then subjected to a fourth classification. The products of felt beneficiation 1 are precious metal concentrate 2 and high-grade nickel-copper concentrate.
[0019] 3) The overflow of the four-stage classification is added with 90g of ethyl xanthate, 280g of ammonium sulfate, and 20g of BQ-622 per ton of raw ore. After two-stage roughing, two-stage cleaning, and felt beneficiation 2 using long-haired gold mining grass material, the middlings from the four-stage classification are returned to the four-stage classification after two-stage grinding. The middlings from the two-stage roughing enter the two-stage scavenging. The middlings from the two-stage cleaning return to the four-stage classification. The products of felt beneficiation 2 are precious metal concentrate 3 and low-grade nickel-copper concentrate.
[0020] 4) The roughing concentrate undergoes a two-stage scavenging process. The tailings from the two-stage scavenging process are then subjected to primary and secondary desliming. The tailings from both processes are discharged into the total tailings. The secondary deslimed concentrate undergoes magnetic separation at a magnetic field strength of 1300 Gauss. The magnetically separated concentrate is then subjected to sluice box beneficiation, and the sluice box beneficiation concentrate is then subjected to felt beneficiation 3. Felt beneficiation 3 uses long-pile gold-digging grass made of low-density polyethylene with a pile height of 13cm. The tailings from primary desliming, secondary desliming, magnetic separation, sluice box beneficiation, and felt beneficiation 3 are combined into a total tailings. The product of felt beneficiation 3 is precious metal concentrate 4. The experimental results are shown in Table 1.
[0021] Table 1 Test Indicators product Gold grade g / t Platinum grade g / t Precious metal concentrate 1 85 247 Precious metal concentrate 2 681 1003 Precious metal concentrate 3 314 437 Precious metal concentrate 4 23 87 Mineral processing according to Figure 2 Steps to be performed: After the -13mm raw ore undergoes a single-stage grinding process, it is subsequently subjected to a first-stage hydrocyclone classification and a second-stage hydrocyclone classification, using the Nelson gravity separation 1 operation. The middlings from the first-stage hydrocyclone classification are returned to the first-stage grinding process. The middlings from the second-stage hydrocyclone classification, consisting of a slurry with a -0.074mm content of 68%, enter the first-stage roughing process. The middlings from the Nelson gravity separation 1 undergo a third-stage classification, and the precipitate from the third-stage classification is then combined with the overflow from the third-stage classification and returned to the second-stage classification process. The product of the Nelson gravity separation 1 is precious metal concentrate 1. The experimental results are shown in Table 2.
[0022] Table 2 Test Indicators product Gold grade g / t Platinum grade g / t Precious metal concentrate 1 81 239 A comparison of the data in Tables 1 and 2 shows that the present invention increases the recovery of precious metals from high-grade concentrate, low-grade concentrate, and tailings, thereby improving the recovery of precious metals.
[0023] Example 2: In this example, the raw ore contains 1.35% nickel and 1.13% copper, and the main gangue mineral is serpentine.
[0024] Mineral processing according to Figure 1 Steps to be performed: 1) After the -13mm raw ore undergoes a first-stage grinding process, it is successively subjected to a first-stage hydrocyclone classification, a second-stage hydrocyclone classification, and the Nelson gravity separation 1 operation. The middlings from the first-stage hydrocyclone classification are returned to the first-stage grinding process. The middlings from the second-stage hydrocyclone classification are slurries with a -0.074mm content of 68% and enter the first-stage roughing process. The middlings from the Nelson gravity separation 1 undergo a third-stage classification process. The underflow from the third-stage classification is then combined with the overflow from the third-stage classification and returned to the second-stage classification process. The product of the Nelson gravity separation 1 is precious metal concentrate 1.
[0025] 2) The middlings from the secondary classification consist of a slurry with a -0.074mm content of 68%. Reagents are added per ton of raw ore: 170g butyl xanthate, 60g ethyl xanthate, 800g ammonium sulfate, and 50g BQ-622. A roughing operation is then performed. The flotation product, without reagent addition, proceeds to a cleaning operation. The cleaning product is then subjected to felt beneficiation 1, using 13mm thick fiber gold panning cloth. The middlings from the primary roughing and cleaning operations are then subjected to a fourth classification. The products of felt beneficiation 1 are precious metal concentrate 2 and high-grade nickel-copper concentrate.
[0026] 3) The overflow of the four-stage classification is added with 90g of ethyl xanthate, 280g of ammonium sulfate, and 20g of BQ-622 per ton of raw ore. After two-stage roughing, two-stage cleaning, and felt beneficiation 2 using long-haired gold mining grass material, the middlings from the four-stage classification are returned to the four-stage classification after two-stage grinding. The middlings from the two-stage roughing enter the two-stage scavenging. The middlings from the two-stage cleaning return to the four-stage classification. The products of felt beneficiation 2 are precious metal concentrate 3 and low-grade nickel-copper concentrate.
[0027] 4) The roughing concentrate undergoes a two-stage scavenging process. The tailings from the two-stage scavenging process are then subjected to primary and secondary desliming. The tailings from both processes are discharged into the total tailings. The secondary deslimed concentrate undergoes magnetic separation at a magnetic field strength of 1300 Gauss. The magnetically separated concentrate is then subjected to sluice box beneficiation, and the sluice box beneficiation concentrate is then subjected to felt beneficiation 3. Felt beneficiation 3 uses long-pile gold-digging grass made of low-density polyethylene with a pile height of 13cm. The tailings from primary desliming, secondary desliming, magnetic separation, sluice box beneficiation, and felt beneficiation 3 are combined into a total tailings. The product of felt beneficiation 3 is precious metal concentrate 4. The test results are shown in Table 3.
[0028] Table 3 Test Indicators product Gold grade g / t Platinum grade g / t Precious metal concentrate 1 58 199 Precious metal concentrate 2 421 712 Precious metal concentrate 3 157 256 Precious metal concentrate 4 14 62 Example 3: In this example, the raw ore contains 1.10% nickel and 0.85% copper, and the main gangue mineral is serpentine.
[0029] Mineral processing according to Figure 1 Steps to be performed: 1) After the -13mm raw ore undergoes a first-stage grinding process, it is successively subjected to a first-stage hydrocyclone classification, a second-stage hydrocyclone classification, and the Nelson gravity separation 1 operation. The middlings from the first-stage hydrocyclone classification are returned to the first-stage grinding process. The middlings from the second-stage hydrocyclone classification are slurries with a -0.074mm content of 68% and enter the first-stage roughing process. The middlings from the Nelson gravity separation 1 undergo a third-stage classification process. The underflow from the third-stage classification is then combined with the overflow from the third-stage classification and returned to the second-stage classification process. The product of the Nelson gravity separation 1 is precious metal concentrate 1.
[0030] 2) The middlings from the secondary classification consist of a slurry with a -0.074mm content of 68%. Reagents are added per ton of raw ore: 170g butyl xanthate, 60g ethyl xanthate, 800g ammonium sulfate, and 50g BQ-622. A roughing operation is then performed. The flotation product, without reagent addition, proceeds to a cleaning operation. The cleaning product is then subjected to felt beneficiation 1, using 13mm thick fiber gold panning cloth. The middlings from the primary roughing and cleaning operations are then subjected to a fourth classification. The products of felt beneficiation 1 are precious metal concentrate 2 and high-grade nickel-copper concentrate.
[0031] 3) The overflow of the four-stage classification is added with 90g of ethyl xanthate, 280g of ammonium sulfate, and 20g of BQ-622 per ton of raw ore. After two-stage roughing, two-stage cleaning, and felt beneficiation 2 using long-haired gold mining grass material, the middlings from the four-stage classification are returned to the four-stage classification after two-stage grinding. The middlings from the two-stage roughing enter the two-stage scavenging. The middlings from the two-stage cleaning return to the four-stage classification. The products of felt beneficiation 2 are precious metal concentrate 3 and low-grade nickel-copper concentrate.
[0032] 4) The roughing concentrate undergoes a two-stage scavenging process. The tailings from the two-stage scavenging process are then subjected to primary and secondary desliming. The tailings from both processes are discharged into the total tailings. The secondary deslimed concentrate undergoes magnetic separation at a magnetic field strength of 1300 Gauss. The magnetically separated concentrate is then subjected to sluice box beneficiation, and the sluice box beneficiation concentrate is then subjected to felt beneficiation 3. Felt beneficiation 3 uses long-pile gold-digging grass made of low-density polyethylene with a pile height of 13cm. The tailings from primary desliming, secondary desliming, magnetic separation, sluice box beneficiation, and felt beneficiation 3 are combined into a total tailings. The product of felt beneficiation 3 is precious metal concentrate 4. The test results are shown in Table 4.
[0033] Table 4 Test Indicators product Gold grade g / t Platinum grade g / t Precious metal concentrate 1 45 150 Precious metal concentrate 2 253 511 Precious metal concentrate 3 124 187 Precious metal concentrate 4 10 41
Claims
1. A mineral processing technology for the complete recovery of precious metals from copper-nickel sulfide ores, characterized in that, Includes the following steps: 1) After the nickel-copper ore is ground once, it is then subjected to primary classification, secondary classification and Nilsson gravity separation 1 operation in sequence; The middlings from the first classification are returned to the first grinding stage, the middlings from the second classification enter the first roughing stage, and the middlings from Nelson gravity separation 1 undergo a third classification. The third-classification underflow is then combined with the third-classification overflow after a second grinding stage and returned to the second classification stage. The product of Nelson gravity separation 1 is precious metal concentrate 1. 2) After the first stage of roughing, a first stage of cleaning and felt beneficiation are carried out in sequence; The middlings from the roughing process and the middlings from the first beneficiation process enter the fourth grading stage. The products of felt beneficiation 1 are precious metal concentrate 2 and high-grade nickel-copper concentrate. 3) After four stages of overflow, two-stage roughing, two-stage cleaning, and felt beneficiation operations are carried out in sequence; Among them, the middlings from the fourth grade are returned to the fourth grade after two stages of grinding; the middlings from the second stage roughing are subjected to a second stage of scavenging; the middlings from the second stage cleaning are returned to the fourth grade; the products of felt beneficiation 2 are precious metal concentrate 3 and low-grade nickel-copper concentrate. 4) The tailings of the two-stage scavenging operation are subjected to three operations in sequence: primary desliming, secondary desliming, magnetic separation, sluice box beneficiation, and felt beneficiation. Among them, the middlings from the second-stage scavenging are returned to the fourth stage of classification. The tailings from the first desliming, second desliming, magnetic separation, sluice box beneficiation, and felt beneficiation 3 are combined into the total tailings. The product of felt beneficiation 3 is precious metal concentrate 4.
2. The beneficiation process for recovering precious metals from copper-nickel sulfide ore according to claim 1, characterized in that, In step 1), the nickel-copper ore particle size is -13mm, the first-stage grinding concentration is 60%, and the first-stage grinding uses steel balls of 90mm, 80mm and 60mm, respectively, in a weight ratio of 3:1:1; the second-stage ball mill uses 50mm*60mm and 35mm*40mm cast iron segments in a weight ratio of 1:
1.
3. The beneficiation process for recovering precious metals from copper-nickel sulfide ore according to claim 1, characterized in that, In step 2), the dosage of butyl xanthate collector in the roughing flotation is 160g / t-180g / t of raw ore, the dosage of ethyl xanthate is 40g / t-80g / t of raw ore, the dosage of ammonium sulfate modifier is 700g / t-800g / t of raw ore, and the dosage of BQ-622 frother is 40-60g / t of raw ore.
4. The beneficiation process for recovering precious metals from copper-nickel sulfide ore according to claim 1, characterized in that, In step 2), the content of the coarse particle size of -0.074mm is 65%-70%. The gold panning cloth used in the felt beneficiation operation is 50cm*300cm, made of fiber, with a pile height of 13mm.
5. The beneficiation process for recovering precious metals from copper-nickel sulfide ore throughout the entire process according to claim 1, characterized in that, In step 3), the content of -0.074mm particles in the second-stage roughing is 80%-85%, the dosage of ethyl xanthate collector in the second-stage roughing flotation reagent is 80g / t-100g / t of raw ore, the dosage of ammonium sulfate modifier is 250g / t-300g / t of raw ore, and the dosage of BQ-622 frother is 10-20g / t of raw ore.
6. The beneficiation process for recovering precious metals from copper-nickel sulfide ore according to claim 1, characterized in that, In step 4), the primary and secondary desliming processes use desliming hydrocyclones, with a feed concentration of 35%-40% and a feed pressure of 0.08-0.12 MPa. The magnetic separation equipment is a wet magnetic separator with a magnetic field strength of 1300 Gauss; For regrinding magnetic concentrate, ceramic balls are used as the grinding media. The ceramic balls are mixed with 25mm, 20mm and 15mm steel balls in a weight ratio of 2:1:
1. The content of -0.074mm in the grinding product accounts for 81%-84% of the total particle size.
Citation Information
Patent Citations
A mineral processing method for recovering polymetals from gold-bearing gravity separation tailings
CN112657670B
Beneficiation method for high-grade copper-nickel sulphide ore
CN103736584A
Beneficiation method for non-uniformly distributed copper-nickel sulfide tailings
CN114643133A