A method for beneficiation of a copper nickel sulphide ore
By employing a two-stage grinding and multiple-stage beneficiation method, the problems of poor enrichment and high flotation difficulty in the beneficiation of low-grade copper-nickel sulfide ores have been solved, achieving efficient recovery of useful minerals and optimizing system processing capacity and concentrate quality.
Patent Information
- Application Number
- CN202410349908.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-26
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-03-26
AI Technical Summary
Existing copper-nickel sulfide ore beneficiation processes suffer from poor enrichment and flotation when processing low-grade ores, resulting in high system loads and difficulty in meeting the requirements of smelting systems for high-grade concentrates. Furthermore, the high magnesium oxide content affects the recovery rate.
A mineral processing method involving two-stage grinding, multiple cleaning and scavenging is adopted. By adjusting the reagent dosage and process flow, easily floatable minerals are floated in stages, reducing the impact of fine gangue, improving the recovery rate of useful minerals, and optimizing the system's processing capacity.
It improved the metal recovery rate and quality of low-grade concentrates, reduced the magnesium oxide content, and enhanced the system's processing capacity and recovery rate.
Smart Images

Figure CN118218123B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a mineral processing method, specifically a mineral processing method for copper-nickel sulfide ore. Background Technology
[0002] With the development of the non-ferrous metals industry and the continuous development and utilization of copper-nickel sulfide ores, the properties of copper-nickel sulfide ores have undergone the following changes: the metal grade of the raw ore has decreased, the magnesium oxide content has increased, and a large amount of easily floatable slime is easily generated during the grinding process, which affects the floatability of copper-nickel minerals, resulting in poor enrichment and concentration. At the same time, the magnesium oxide grade of the concentrate has increased, leading to increased flotation difficulty.
[0003] Taking a large-scale copper-nickel sulfide ore beneficiation process as an example, it employs two-stage grinding, two-stage roughing, multiple cleaning stages, and rough scavenging to produce two products: high-grade concentrate and low-grade concentrate. This process is effective for beneficiating copper-nickel sulfide ores with high grade and hardness. However, with continuous mining and utilization, mineral resources are trending towards leaner, finer, more complex, and more difficult-to-process ore. While maintaining high-grade concentrate quality, the yield of the first-stage high-grade concentrate is continuously declining, leading to an increase in the feed rate to the second-stage flotation, increasing the system load and reducing the system's processing capacity. Simultaneously, because the flash furnace in the smelting system requires a magnesium oxide content of ≤7.5% in the high-grade concentrate, and the oxygen-enriched top-blown furnace requires a magnesium oxide content of ≤13.0% in the low-grade concentrate, it is necessary to improve the original beneficiation process to reduce the feed rate to the second-stage flotation, optimize the second-stage flotation environment, reduce the system load, increase the system's processing capacity, improve the quality of the low-grade concentrate, reduce the magnesium oxide content in the low-grade concentrate, and increase the nickel recovery rate. Summary of the Invention
[0004] To address the shortcomings of existing technologies, this invention provides a beneficiation method for copper-nickel sulfide ores, which improves the metal recovery rate of copper-nickel sulfide ores, enhances the quality of low-grade concentrates, reduces the magnesium oxide content in the concentrates, reduces system load, and increases system processing capacity.
[0005] This invention is achieved through the following scheme: (1) After the raw ore is ground in one stage, it is roughed in one stage. The tailings of the roughing in one stage are ground again and then roughed and scavenged in one stage. The concentrate of the roughing in one stage is cleaned twice. The concentrate of the first stage of the first stage of the first stage of the first stage of the first stage of the first stage of the second stage of the first ... (2) The roughing concentrate of the second stage is cleaned twice. The concentrate of the first stage of the second stage enters the second stage of ... (3) After the tailings of the second stage roughing and the tailings of the first stage roughing are combined, two scavenging operations are carried out. The tailings of the first stage scavenging enter the second stage scavenging, and the concentrate of the second stage scavenging is returned to the previous stage. The tailings of the second stage scavenging are the final tailings.
[0006] In step (1) above, the raw ore is a low-grade copper-nickel sulfide ore containing less than 3% nickel. After the first grinding stage, the content of the grinding product below -200 mesh accounts for 60% to 65% of the total particle size. During the first roughing stage, the dosage of the modifier ammonium sulfate is 270 to 330 g / t, the dosage of the collector ethyl xanthate is 100 to 140 g / t, and the dosage of the frother butylammonium black is 15 to 45 g / t. During the first cleaning stage, the dosage of the magnesium-reducing agent sodium hexametaphosphate is 0 to 80 g / t. After entering the first roughing and tailings scavenging stage, the content of the grinding product below -200 mesh accounts for 80% to 85% of the total particle size. The dosage of the collector ethyl xanthate is 60 to 100 g / t, and the dosage of the frother butylammonium black is 15 to 45 g / t. In step (2) above, the content of the grinding product below -200 mesh in the second stage roughing process accounts for 80%~85% of the total particle size, and the amount of collector ethyl xanthate is 80~120g / t.
[0007] In step (3) above, during the second-stage scavenging, the amount of ethyl xanthate collector used is 60~80g / t.
[0008] Compared with the prior art, the present invention has the following advantages: By employing staged flotation, the first stage recovers easily floatable copper-nickel minerals, while the tailings from the first stage roughing are regrinded and then scavenged. This pre-enrichment of the first-stage roughing tailings removes some muddy gangue, reducing the impact of fine-grained gangue on the second-stage flotation and improving the floating environment for valuable minerals. The second stage involves fine grinding to fully liberate the valuable minerals, further recovering the copper-nickel sulfide ores that are difficult to flotate in the fine-grained stage. Attached Figure Description
[0009] Figure 1 This is a traditional process flow diagram; Figure 2 This is a process flow diagram of the present invention. Detailed Implementation
[0010] The present invention will be further explained and described below with reference to specific embodiments.
[0011] The ore sample is a sample from a copper-nickel sulfide mine in Jinchuan. The raw ore contains 0.73% nickel and 0.39% copper. The nickel minerals are mainly nickel pyrite and trace amounts of purpurite, while the copper minerals are mainly chalcopyrite, chalcopyrite and trace amounts of chalcopyrite. The main gangue minerals are serpentine, pyroxene, olivine, etc.
[0012] Comparative Example 1 The above ore samples were arranged according to Figure 1 The mineral processing procedure shown is as follows: (1) The crushed and qualified ore samples are sent to a first-stage closed-circuit grinding and classification process consisting of a hydrocyclone and a ball mill for grinding and classification. The first-stage grinding concentration is 65%, the second-stage grinding concentration is 70%, and the grinding fineness is -200 mesh, accounting for 65%. The slurry after grinding and classification is fed into a mixing tank, and modifier, collector and frother are added and stirred evenly before first-stage roughing. The first-stage roughing concentration is 33%, the flotation reagents are ammonium sulfate 300g / t, ethyl xanthate 120g / t, and frother 35g / t. Then, 30g / t of magnesium-reducing reagent sodium hexametaphosphate is added to the first-stage roughing concentrate for two-stage cleaning. The first-stage cleaning concentration is 11%, and the first-stage cleaning concentrate enters the first-stage second-stage cleaning. The first-stage second-stage cleaning concentration is 13%, and the tailings of the first-stage second-stage cleaning are returned to the previous stage. The first-stage second-stage cleaning concentrate is the high-grade concentrate. The tailings from the first stage roughing, the first stage primary cleaning, the second stage primary cleaning, and the second stage primary scavenging concentrate are pumped into a two-stage closed-circuit grinding and classification process consisting of a hydrocyclone and a ball mill for grinding and classification. The grinding concentration is 72%, and the grinding fineness is such that the content below -200 mesh accounts for 85% of the total particle size. The slurry after grinding and classification is fed into a mixing tank, and after adding a frother and stirring evenly, it is subjected to second-stage roughing. The second-stage roughing concentration is 23%, and the flotation reagent collector ethyl xanthate dosage is 96 g / t.
[0013] (2) The roughing concentrate of the second stage is cleaned twice. The concentration of the first cleaning in the second stage is 9%. The concentrate of the first cleaning in the second stage enters the second cleaning in the second stage. The concentration of the second cleaning in the second stage is 10%. The concentrate of the second cleaning in the second stage is the low-grade concentrate. The tailings of the second cleaning in the second stage are returned to the previous stage. (3) The tailings from the second-stage roughing and the tailings from the first-stage roughing scavenging are combined and then subjected to two scavenging operations. The concentration of the first scavenging in the second stage is 19%, and the amount of ethyl xanthate collector is 68 g / t. The tailings from the first scavenging in the second stage enter the second scavenging in the second stage, and the concentration of the second scavenging in the second stage is 16%. The concentrate from the second scavenging in the second stage is returned to the previous stage, and the tailings from the second scavenging in the second stage are the final tailings. The test results are shown in Table 1.
[0014] Table 1 Example 1 The above ore samples were arranged according to Figure 2 The mineral processing procedure shown is as follows: (1) The crushed and qualified ore samples are sent to a first-stage closed-circuit grinding and classification process consisting of a hydrocyclone and a ball mill for grinding and classification. The first-stage grinding concentration is 65%, the second-stage grinding concentration is 70%, and the grinding fineness is -200 mesh, accounting for 65%. The slurry after grinding and classification is fed into a mixing tank, and modifier, collector and frother are added and stirred evenly before first-stage roughing. The first-stage roughing concentration is 33%, the flotation reagents are ammonium sulfate 300g / t, ethyl xanthate 120g / t, and frother 35g / t. Then, 30g / t of magnesium-reducing reagent sodium hexametaphosphate is added to the first-stage roughing concentrate for two-stage cleaning. The first-stage cleaning concentration is 11%, and the first-stage cleaning concentrate enters the first-stage second-stage cleaning. The first-stage second-stage cleaning concentration is 13%, and the tailings of the first-stage second-stage cleaning are returned to the previous stage. The first-stage second-stage cleaning concentrate is the high-grade concentrate. The roughing tailings are pumped to a ball mill for regrinding and then subjected to roughing tailings scavenging. The content of the grinding product below -200 mesh accounts for 85% of the total particle size. The flotation reagents, collector ethyl xanthate, are used at a rate of 80 g / t, and frother butyl ammonium black is used at a rate of 35 g / t. The tailings from the first stage of primary beneficiation, the tailings from the second stage of primary beneficiation, and the concentrate from the second stage of primary scavenging are pumped to a two-stage closed-circuit grinding and classification process consisting of a hydrocyclone and a ball mill for grinding and classification. The grinding concentration is 72%, and the grinding fineness is such that the content below -200 mesh accounts for 85% of the total particle size. The slurry after grinding and classification is combined with the scavenging concentrate from the first stage of coarse tailings and fed into a mixing tank. After adding a frother and stirring evenly, the second stage of roughing is carried out. The concentration of the second stage roughing is 23%, and the dosage of the flotation reagent collector ethyl xanthate is 96 g / t.
[0015] (2) The roughing concentrate of the second stage is cleaned twice. The concentration of the first cleaning in the second stage is 9%. The concentrate of the first cleaning in the second stage enters the second cleaning in the second stage. The concentration of the second cleaning in the second stage is 10%. The concentrate of the second cleaning in the second stage is the low-grade concentrate. The tailings of the second cleaning in the second stage are returned to the previous stage. (3) The tailings from the second-stage roughing and the tailings from the first-stage roughing scavenging are combined and then subjected to two scavenging operations. The concentration of the first scavenging in the second stage is 19%, and the amount of ethyl xanthate collector is 68 g / t. The tailings from the first scavenging in the second stage enter the second scavenging in the second stage, and the concentration of the second scavenging in the second stage is 16%. The concentrate from the second scavenging in the second stage is returned to the previous stage, and the tailings from the second scavenging in the second stage are the final tailings. The test results are shown in Table 2.
[0016] Table 2 As can be seen from the comparison of the data in Tables 1 and 2, the mineral processing method provided by the present invention, compared with the traditional mineral processing method, increases the low-grade nickel content by 0.24%, decreases the low-grade magnesium oxide content by 2.52%, increases the nickel recovery rate by 3.26%, and increases the copper recovery rate by 3.55%.
Claims
1. A beneficiation method of copper nickel sulfide ore, characterized by, Includes the following steps: (1) After the raw ore is ground in one stage, it is roughed in one stage. The tailings of the roughing in one stage are ground again and then roughed and scavenged in one stage. The concentrate of the roughing in one stage is cleaned twice. The concentrate of the first stage of the first stage of the first stage of the first stage of the first stage of the first stage of the second stage of the first ... (2) The roughing concentrate of the second stage is cleaned twice. The concentrate of the first stage of the second stage enters the second stage of ... (3) After the tailings of the second stage roughing and the tailings of the first stage roughing are combined, two scavenging operations are carried out. The tailings of the first stage scavenging enter the second stage scavenging, and the concentrate of the second stage scavenging is returned to the previous stage. The tailings of the second stage scavenging are the final tailings.
2. The beneficiation method for copper-nickel sulfide ore as described in claim 1, characterized in that, In step (1), the raw ore is a copper-nickel sulfide ore containing less than 3% nickel, and the content of the grinding product below -200 mesh after the first grinding stage accounts for 60% to 65% of the total particle size.
3. The beneficiation method for copper-nickel sulfide ore as described in claim 1, characterized in that, In step (1), during the first coarse separation, the amount of ammonium sulfate as the modifier is 270~330g / t, the amount of ethyl xanthate as the collector is 100~140g / t, and the amount of butyl ammonium black powder as the frother is 15~45g / t.
4. The beneficiation method for copper-nickel sulfide ore as described in claim 1, characterized in that, In step (1), during the first-stage selection, the dosage of sodium hexametaphosphate, a magnesium-lowering agent, is 0~80g / t.
5. The beneficiation method for copper-nickel sulfide ore as described in claim 1, characterized in that, In step (1), the content of the grinding product below -200 mesh in the coarse tailings scavenging process accounts for 80%~85% of the total particle size. The amount of collector ethyl xanthate is 60~100g / t, and the amount of frother butylammonium black is 15~45g / t.
6. The beneficiation method for copper-nickel sulfide ore as described in claim 1, characterized in that, In step (1), the content of the grinding product below -200 mesh in the second stage roughing process accounts for 80%~85% of the total particle size, and the amount of collector ethyl xanthate is 80~120g / t.
7. The beneficiation method for copper-nickel sulfide ore as described in claim 1, characterized in that, In step (3), during the second-stage single-stage scavenging, the amount of ethyl xanthate collector used is 60~80g / t.
Citation Information
Patent Citations
Dressing-metallurgy combined method for treating ultra-fine copper sulfide ore
CN110449270A
Beneficiation method for copper-nickel sulfide ore
CN112474030A