A method for rough and fine separation of a nickel-copper sulfide ore
By employing a dual overflow hydrocyclone classification process and multiple fine scavenging column flotation processes, the problem of separating fine-grained minerals has been solved, enabling efficient recovery of valuable metals and efficient utilization of resources.
Patent Information
- Application Number
- CN202410349916.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-26
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-03-26
AI Technical Summary
In existing technologies, fine-grained minerals are difficult to separate during flotation, leading to the loss of valuable metals, affecting separation efficiency and resource utilization. Furthermore, flotation equipment is not effective at separating fine particles.
A dual overflow hydrocyclone is used to classify the slurry, producing two overflow products of different fineness. These products are then selectively separated in a flotation machine and a flotation column, respectively. This combined process of multiple fine scavenging and column flotation improves the recovery rate of fine particles.
It improved the recovery rate of valuable metals, reduced the grade of tailings, decreased the amount of fine particles recycled, improved flotation efficiency, provided qualified smelting raw materials, and improved resource utilization.
Smart Images

Figure CN118218124B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of non-ferrous metal mineral beneficiation technology, and relates to a method for coarse and fine separation of nickel-copper sulfide ore. Background Technology
[0002] Many factors influence flotation efficiency, including feed concentration, fineness, reagent formulation, aeration rate, and flotation time. Feed fineness is a key factor; for ores with high fine particle content after grinding and classification, excessive mudding is detrimental to the flotation process. Currently, most hydrocyclones used in mineral processing typically produce only one overflow product, which enters the flotation machine or column for further separation. This separation lacks specificity, resulting in a low content of easily separable particle sizes. Furthermore, the separation efficiency of flotation machines for fine particles is relatively lower than that of flotation columns. Some of the difficult-to-separate fine particles continuously circulate in the process, while others are lost with the tailings, impacting separation efficiency, causing significant loss of valuable metals, and reducing mineral resource utilization.
[0003] Meanwhile, in mineral processing, crushing and grinding inevitably produce a large number of fine mineral particles smaller than 10 micrometers. Due to their high surface energy, these fine mineral particles, under certain conditions, are prone to non-selective agglomeration between particles of different compositions. Furthermore, while fine mineral particles have high adsorption capacity for reagents, their selective adsorption is poor, and their surface solubility is high, leading to an increase in the number of difficult-to-separate fine mineral particles in the pulp. The small size of these fine mineral particles also reduces their likelihood of collision with flotation bubbles. Because of their small size, they cannot overcome the resistance of the hydration layer between the mineral particles and bubbles when they collide, making it difficult for them to adhere to the bubbles and preventing the separation of valuable minerals from gangue minerals. Therefore, fine mineral particles are detrimental to flotation, resulting in a large number of fine particles not being effectively separated during the flotation process, thus being lost in the tailings or continuously recycled in the process, severely affecting the effectiveness and efficiency of the flotation operation. Summary of the Invention
[0004] The purpose of this invention is to address the problems existing in the prior art by providing a method for coarse and fine separation of nickel-copper sulfide ore. This method utilizes a double overflow hydrocyclone to classify the ore into two overflow products with different finenesses. Then, based on the different characteristics of the two overflow products, different separation equipment is used for targeted separation, thereby solving the problems in the prior art.
[0005] Therefore, the present invention adopts the following technical solution: A method for coarse and fine separation of nickel-copper sulfide ore includes the following steps: After the raw ore is ground, a slurry is formed and fed into a double overflow hydrocyclone. The slurry is classified by the double overflow hydrocyclone to produce coarser underflow, finer outflow slurry, and finer inflow slurry. The underflow is returned to the grinding operation for re-grinding, forming a closed loop with the grinding operation. The outflow slurry is fed into a flotation machine for one roughing operation, two cleaning operations, two fine scavenging operations, and two scavenging operations. The inflow slurry is fed into a flotation column for two column flotation separation operations.
[0006] Furthermore, the working concentration of the grinding operation is 68% ± 2%, and more preferably 66%, 68%, or 70%.
[0007] Furthermore, the proportion of 200-mesh fineness slurry in the external overflow hydrocyclone is 78-82%, more preferably 78%, 80%, or 83%; the concentration of the external overflow slurry is 25-27%, more preferably 25%, 26%, or 27%; and the proportion of 200-mesh fineness slurry in the internal overflow hydrocyclone is 88-92%, more preferably 88%, 90%, or 92%.
[0008] Furthermore, the primary roughing operation includes adjusting the pH of the slurry with a modifier, and then sequentially adding an inhibitor, an activator, a collector, and a frother to obtain a rough concentrate and rough tailings; Specifically, in the primary roughing process, the adjusting agent is ammonium sulfate, and the dosage of ammonium sulfate is 240-300 g / t, more preferably 240 g / t, 250 g / t, 260 g / t, 270 g / t, 280 g / t, 290 g / t, or 300 g / t, and even more preferably 260 g / t, 270 g / t, or 280 g / t, to adjust the pulp pH to 9-10; the activator is copper sulfate, and the dosage of copper sulfate is 9-11 g / t, more preferably 9 g / t, 10 g / t, or 11 g / t; the inhibitor is sodium hexametaphosphate, and the dosage of sodium hexametaphosphate is 70-90 g / t, more preferably 70 g / t, 80 g / t, or 9 ... 90 g / t; the collector is butyl xanthate, and the dosage of butyl xanthate is 60-70 g / t, more preferably 60 g / t, 65 g / t, or 70 g / t; the foaming agent is BQ-622, which is prepared by BQz, BQA, and MIBC foaming agents in a certain proportion, and the dosage of BQ-622 is 6-10 g / t, more preferably 6 g / t, 8 g / t, or 10 g / t; the collector foaming agent BQz is synthesized by diethylaminodithiocarbamate, n-butyl xanthoxypropionitrile, etc. in a certain proportion, and the main component of the collector foaming agent BQ-622 is N-allyl-O-alkylthiocarbamate.
[0009] Furthermore, the two refining operations include a primary refining operation and a secondary refining operation. The rough concentrate enters the primary refining operation, which yields a primary refined concentrate and a primary refined tailings. The primary refined concentrate enters the secondary refining operation, which yields a secondary refined concentrate and a secondary refined tailings.
[0010] Furthermore, the two fine scavenging operations include a primary fine scavenging operation and a secondary fine scavenging operation. The primary fine scavenging operation yields a primary fine scavenging concentrate and a primary fine scavenging tailings. The secondary fine scavenging concentrate is returned to the secondary cleaning operation. The primary fine scavenging concentrate and the secondary fine scavenging tailings are returned to the primary cleaning operation. The primary cleaning tailings obtained from the primary cleaning operation enter the primary fine scavenging operation. The secondary cleaning operation yields a secondary cleaning concentrate and a secondary cleaning tailings, and the secondary cleaning tailings are returned to the primary cleaning operation.
[0011] Furthermore, the two scavenging operations include a primary scavenging operation and a secondary scavenging operation; wherein, the primary scavenging operation includes: adjusting the pH of the slurry with a regulator, then adding a collector to obtain a primary scavenging concentrate and a primary scavenging tailings, the primary scavenging concentrate entering the secondary scavenging operation, the secondary scavenging operation obtaining a secondary scavenging concentrate and total tailings, the primary scavenging concentrate and secondary scavenging concentrate and the primary fine scavenging tailings being combined and returned to the primary roughing process.
[0012] Specifically, the modifier in the primary scavenging process is ammonium sulfate, and the dosage of ammonium sulfate is 90-110 g / t, more preferably 90 g / t, 100 g / t, or 110 g / t, to adjust the pH of the pulp to 9-10; the collector is butyl xanthate, and the dosage of butyl xanthate is 20-30 g / t, more preferably 20 g / t, 25 g / t, or 30 g / t.
[0013] Furthermore, the two column flotation separation operations include a primary column flotation operation and a secondary column flotation operation; wherein, the primary column flotation operation yields a primary column flotation concentrate and a primary column flotation tailings, the primary column flotation concentrate enters a flotation column for a secondary column flotation operation, and the primary column flotation tailings are returned to a primary scavenging operation; the secondary column flotation operation yields a secondary column flotation concentrate and a secondary column flotation tailings, the secondary column flotation concentrate is combined with the concentrate from the secondary cleaning operation as the final concentrate product, and the secondary column flotation tailings are returned to the primary column flotation operation.
[0014] The beneficial effects of this invention are as follows: 1. This invention utilizes the characteristic of a dual overflow hydrocyclone that can produce two overflow products with different finenesses to separate fine particles in the slurry after grinding from the traditional single overflow product. The overflow slurry with a lower content of fine particles has a higher recovery rate of valuable metals and a lower tailings grade during the flotation process using a flotation machine. The amount of fine particles circulating in the process is reduced, which reduces the impact on the flotation process and improves the flotation efficiency. 2. Flotation columns are generally considered by the mineral processing industry to be more suitable for separating fine-grained minerals. In this invention, the internal overflow slurry product with higher fine-grained content, which is classified by the double overflow hydrocyclone, is targeted for separation using a flotation column. This can maximize the recovery of valuable metals in the fine particles and avoid the loss of metals due to the inability to effectively separate the valuable metals in these fine particles. 3. This invention addresses the problem of the impact of fine-grained ores that is common in the mineral processing industry by proposing the concept of coarse-grained separation. It provides a new approach to beneficiation for similar enterprises in the non-ferrous metals industry that are troubled by mud formation, thereby increasing the possibility of recovering various non-ferrous metal fine particles. 4. This invention yields a copper-nickel mixed concentrate with qualified concentrate grade, providing qualified raw materials for the smelting system and maximizing resource utilization. When the nickel grade of the raw ore is 0.45%–0.50%, the concentrate nickel grade can reach 4.5%–5.0%, the tailings nickel grade is 0.18%–0.19%, and the nickel recovery rate can reach 62%–66%. The nickel metal content of the tailings from the sulfide nickel-copper ore beneficiation process after this process is reduced by 0.02% compared to the beneficiation methods of ordinary hydrocyclones and ordinary flotation machines, and the nickel recovery rate is increased by 4%. Attached Figure Description
[0015] Figure 1 This is a schematic diagram of the process flow of the present invention. Detailed Implementation
[0016] The technical solution of the present invention will be described below with reference to the accompanying drawings and implementation methods.
[0017] Example 1 like Figure 1 As shown, a method for coarse and fine separation of nickel-copper sulfide ore is described. The raw ore is ground at a grinding concentration of 66% to form a slurry. The slurry after grinding is fed into a double overflow hydrocyclone. The sand after classification by the double overflow hydrocyclone is returned to the grinding operation for re-grinding, forming a closed loop with the grinding operation. After classification by the double overflow hydrocyclone, two products are formed: an external overflow slurry with a fineness of 200 mesh (78%) and a concentration of 25% and an internal overflow slurry with a fineness of 200 mesh (92%). The external overflow slurry is fed into a flotation machine for one roughing, two cleaning, two fine scavenging, and two scavenging operations. The internal overflow slurry is fed into a flotation column for two column flotation separation operations.
[0018] The two selection processes are referred to as the first selection process and the second selection process.
[0019] The two fine cleaning operations are a first fine cleaning operation and a second fine cleaning operation.
[0020] The primary roughing operation includes: adjusting the pH of the pulp to 9 with 260 g / t ammonium sulfate, then sequentially adding 70 g / t of sodium hexametaphosphate inhibitor, 9 g / t of copper sulfate activator, 60 g / t of butyl xanthate collector, and 6 g / t of frother BQ-622 to obtain rough concentrate and rough tailings, and the rough concentrate enters the primary cleaning operation.
[0021] The primary concentrate obtained from the primary refining operation enters the secondary refining operation, and the primary tailings obtained from the primary refining operation enter the primary fine scavenging operation.
[0022] The secondary refining operation yields secondary refined concentrate and secondary refined tailings, with the secondary refined tailings being returned to the primary refining operation.
[0023] The first fine scavenging operation yields a first fine scavenging concentrate and a first fine scavenging tailings.
[0024] The secondary scavenging operation yields secondary scavenging concentrate and secondary scavenging tailings. The secondary scavenging concentrate is returned to the secondary cleaning operation, and the primary scavenging concentrate and secondary scavenging tailings are returned to the primary cleaning operation.
[0025] The coarse tailings obtained from the first roughing operation are subjected to two scavenging processes.
[0026] The two scanning operations include a primary scanning operation and a secondary scanning operation.
[0027] The primary scavenging operation includes: adjusting the pH of the slurry to 9 with 90 g / t ammonium sulfate, and then adding 20 g / t of butyl xanthate as a collector to obtain primary scavenging concentrate and primary scavenging tailings. The primary scavenging concentrate then enters the secondary scavenging operation.
[0028] The secondary scavenging operation yields secondary scavenging concentrate and total tailings. The primary scavenging concentrate, secondary scavenging concentrate, and primary fine scavenging tailings are combined and returned to the primary roughing process.
[0029] The overflow slurry from the double overflow hydrocyclone is fed into the first flotation column for primary column flotation. The primary column flotation yields primary column flotation concentrate and primary column flotation tailings. The primary column flotation concentrate enters the second flotation column for secondary column flotation. The primary column flotation tailings are returned to the primary scavenging operation. The secondary column flotation yields secondary column flotation concentrate and secondary column flotation tailings. The secondary column flotation concentrate and the concentrate from the secondary cleaning operation are combined as the final concentrate product. The secondary column flotation tailings are returned to the primary column flotation operation.
[0030] In this embodiment, the nickel grade of the raw ore is 0.45%, the nickel grade of the final concentrate product is 4.5%, the nickel grade of the total tailings is 0.18%, and the nickel recovery rate is 62.50%.
[0031] Example 2 The raw ore is ground to a grinding concentration of 68% to form a slurry. The slurry after grinding is fed into a double overflow hydrocyclone. The sand after classification by the double overflow hydrocyclone is returned to the grinding operation for re-grinding, forming a closed loop with the grinding operation. After classification by the double overflow hydrocyclone, two products are formed: an external overflow slurry with a fineness of 200 mesh (80%) and a concentration of 26% and an internal overflow slurry with a fineness of 200 mesh (90%). The external overflow slurry is fed into a flotation machine for one roughing, two cleaning, two fine scavenging, and two scavenging operations. The internal overflow slurry is fed into a flotation column for two column flotation separation operations.
[0032] The two selection processes are referred to as the first selection process and the second selection process.
[0033] The two fine cleaning operations are a first fine cleaning operation and a second fine cleaning operation.
[0034] The primary roughing operation includes: adjusting the pH of the pulp to 9 using 270 g / t ammonium sulfate, then sequentially adding 80 g / t of sodium hexametaphosphate inhibitor, 10 g / t of copper sulfate activator, 65 g / t of butyl xanthate collector, and 8 g / t of frother BQ-622 to obtain rough concentrate and rough tailings; the rough concentrate then enters the primary cleaning operation.
[0035] The primary concentrate obtained from the primary refining operation enters the secondary refining operation, and the primary tailings obtained from the primary refining operation enter the primary fine scavenging operation.
[0036] The secondary refining operation yields secondary refined concentrate and secondary refined tailings, with the secondary refined tailings being returned to the primary refining operation.
[0037] The first fine scavenging operation yields a first fine scavenging concentrate and a first fine scavenging tailings.
[0038] The secondary scavenging operation yields secondary scavenging concentrate and secondary scavenging tailings. The secondary scavenging concentrate is returned to the secondary cleaning operation, and the primary scavenging concentrate and secondary scavenging tailings are returned to the primary cleaning operation.
[0039] The coarse tailings obtained from the first roughing operation are subjected to two scavenging processes.
[0040] The two scanning operations include a primary scanning operation and a secondary scanning operation.
[0041] The primary scavenging operation includes: adjusting the pH of the slurry to 10 with 100 g / t ammonium sulfate, and then adding 25 g / t of butyl xanthate as a collector to obtain primary scavenging concentrate and primary scavenging tailings. The primary scavenging concentrate then enters the secondary scavenging operation.
[0042] The secondary scavenging operation yields secondary scavenging concentrate and total tailings. The primary scavenging concentrate, secondary scavenging concentrate, and primary fine scavenging tailings are combined and returned to the primary roughing process.
[0043] The overflow slurry in the dual overflow hydrocyclone is fed into the first flotation column for primary column flotation. The primary column flotation yields primary column flotation concentrate and primary column flotation tailings. The primary column flotation concentrate enters the second flotation column for secondary column flotation. The primary column flotation tailings are returned to the primary scavenging operation. The secondary column flotation yields secondary column flotation concentrate and secondary column flotation tailings. The secondary column flotation concentrate and the concentrate from the secondary cleaning operation are combined as the final concentrate product. The secondary column flotation tailings are returned to the primary column flotation operation.
[0044] In this embodiment, the nickel grade of the raw ore is 0.48%, the nickel grade of the final concentrate product is 4.6%, the nickel grade of the total tailings is 0.18%, and the nickel recovery rate is 65.05%.
[0045] Example 3 The raw ore is ground to a grinding concentration of 70% to form a slurry. The slurry after grinding is fed into a double overflow hydrocyclone. The sand after classification by the double overflow hydrocyclone is returned to the grinding operation for re-grinding, forming a closed loop with the grinding operation. After classification by the double overflow hydrocyclone, two products are formed: an external overflow slurry with a fineness of 200 mesh (82%) and a concentration of 27% and an internal overflow slurry with a fineness of 200 mesh (88%). The external overflow slurry is fed into a flotation machine for one roughing, two cleaning, two fine scavenging, and two scavenging operations. The internal overflow slurry is fed into a flotation column for two column flotation operations.
[0046] The two selection processes are referred to as the first selection process and the second selection process.
[0047] The two fine cleaning operations are a first fine cleaning operation and a second fine cleaning operation.
[0048] The primary roughing operation includes: adjusting the pH of the pulp to 10 with 280 g / t ammonium sulfate, then sequentially adding 90 g / t of sodium hexametaphosphate inhibitor, 11 g / t of copper sulfate activator, 70 g / t of butyl xanthate collector, and 10 g / t of BQ-622 frother to obtain rough concentrate and rough tailings; the rough concentrate then enters the primary cleaning operation.
[0049] The primary concentrate obtained from the primary refining operation enters the secondary refining operation, and the primary tailings obtained from the primary refining operation enter the primary fine scavenging operation.
[0050] The secondary refining operation yields secondary refined concentrate and secondary refined tailings, with the secondary refined tailings being returned to the primary refining operation.
[0051] The first fine scavenging operation yields a first fine scavenging concentrate and a first fine scavenging tailings.
[0052] The secondary scavenging operation yields secondary scavenging concentrate and secondary scavenging tailings. The secondary scavenging concentrate is returned to the secondary cleaning operation, and the primary scavenging concentrate and secondary scavenging tailings are returned to the primary cleaning operation.
[0053] The coarse tailings obtained from the first roughing operation are subjected to two scavenging processes.
[0054] The two scanning operations include a primary scanning operation and a secondary scanning operation.
[0055] The primary scavenging operation includes: adjusting the pH of the slurry to 10 with 110 g / t ammonium sulfate, and then adding 30 g / t of butyl xanthate as a collector to obtain primary scavenging concentrate and primary scavenging tailings. The primary scavenging concentrate then enters the secondary scavenging operation.
[0056] The secondary scavenging operation yields secondary scavenging concentrate and total tailings. The primary scavenging concentrate, secondary scavenging concentrate, and primary fine scavenging tailings are combined and returned to the primary roughing process.
[0057] The overflow slurry in the dual overflow hydrocyclone is fed into the first flotation column for primary column flotation. The primary column flotation yields primary column flotation concentrate and primary column flotation tailings. The primary column flotation concentrate enters the second flotation column for secondary column flotation. The primary column flotation tailings are returned to the primary scavenging operation. The secondary column flotation yields secondary column flotation concentrate and secondary column flotation tailings. The secondary column flotation concentrate and the concentrate from the secondary cleaning operation are combined as the final concentrate product. The secondary column flotation tailings are returned to the primary column flotation operation.
[0058] In this embodiment, the nickel grade of the raw ore is 0.50%, the nickel grade of the final concentrate product is 4.9%, the nickel grade of the total tailings is 0.19%, and the nickel recovery rate is 64.50%.
Claims
1. A method for coarse and fine separation of nickel-copper sulfide ore, characterized in that, Includes the following steps: After the raw ore undergoes grinding, a slurry is formed and fed into a double overflow hydrocyclone. The slurry is classified by the double overflow hydrocyclone to produce coarser underflow, finer outflow slurry, and finer inflow slurry. The underflow is returned to the grinding operation for re-grinding, forming a closed loop with the grinding operation. The outflow slurry is fed into a flotation machine for one roughing operation, two cleaning operations, two fine scavenging operations, and two scavenging operations. The inflow slurry is fed into a flotation column for two column flotation separation operations. The two column flotation separation operations include a primary column flotation operation and a secondary column flotation operation; The primary column flotation operation yields primary column flotation concentrate and primary column flotation tailings. The primary column flotation concentrate enters a flotation column for secondary column flotation, and the primary column flotation tailings are returned to a primary scavenging operation. The secondary column flotation operation yields secondary column flotation concentrate and secondary column flotation tailings. The secondary column flotation concentrate and the secondary refined concentrate are combined as the final concentrate product, and the secondary column flotation tailings are returned to the primary column flotation operation.
2. The beneficiation method for coarse and fine separation of nickel-copper sulfide ore according to claim 1, characterized in that, The primary roughing operation includes: adjusting the pH of the slurry with a modifier, and then sequentially adding an inhibitor, an activator, a collector, and a frother to obtain a rough concentrate and rough tailings; In the primary roughing process, the modifier is ammonium sulfate, with a dosage of 240–300 g / t, adjusting the pulp pH to 9–10; the activator is copper sulfate, with a dosage of 9–11 g / t; the inhibitor is sodium hexametaphosphate, with a dosage of 70–90 g / t; the collector is butyl xanthate, with a dosage of 60–70 g / t; and the frother is BQ-622, with a dosage of 6–10 g / t.
3. The method for coarse and fine separation of nickel-copper sulfide ore according to claim 2, characterized in that, The two refining operations include a primary refining operation and a secondary refining operation. The rough concentrate enters the primary refining operation, which yields a primary refined concentrate and a primary refined tailings. The primary refined concentrate enters the secondary refining operation, which yields a secondary refined concentrate and a secondary refined tailings.
4. The beneficiation method for coarse and fine separation of nickel-copper sulfide ore according to claim 3, characterized in that, The two fine scavenging operations include a primary fine scavenging operation and a secondary fine scavenging operation. The primary fine scavenging operation yields a primary fine scavenging concentrate and a primary fine scavenging tailings. The secondary fine scavenging concentrate is returned to the secondary cleaning operation. The primary fine scavenging concentrate and the secondary fine scavenging tailings are returned to the primary cleaning operation. The primary cleaning tailings obtained from the primary cleaning operation are then entered into the primary fine scavenging operation. The secondary cleaning operation yields a secondary cleaning concentrate and a secondary cleaning tailings, and the secondary cleaning tailings are returned to the primary cleaning operation.
5. The method for coarse and fine separation of nickel-copper sulfide ore according to claim 4, characterized in that, The two scavenging operations include a primary scavenging operation and a secondary scavenging operation. The primary scavenging operation includes: adjusting the pH of the slurry with a regulator, then adding a collector to obtain a primary scavenging concentrate and a primary scavenging tailings. The primary scavenging concentrate enters the secondary scavenging operation, which yields a secondary scavenging concentrate and total tailings. The primary scavenging concentrate, the secondary scavenging concentrate, and the primary fine scavenging tailings are combined and returned to the primary roughing process.
6. The beneficiation method for coarse and fine separation of nickel-copper sulfide ore according to claim 1, characterized in that, The overflow slurry from the dual overflow hydrocyclone has a fineness of 200 mesh accounting for 78-82%, and the concentration of the overflow slurry is 25-27%.
7. The method for coarse and fine separation of nickel-copper sulfide ore according to claim 5, characterized in that, The modifier used in the primary scavenging process is ammonium sulfate, with a dosage of 90-110 g / t, to adjust the pulp pH to 9-10; the collector is butyl xanthate, with a dosage of 20-30 g / t.
8. The method for coarse and fine separation of nickel-copper sulfide ore according to claim 1, characterized in that, The proportion of 200-mesh fineness slurry in the double overflow hydrocyclone is 88-92%.
9. The method for coarse and fine separation of nickel-copper sulfide ore according to claim 1, characterized in that, The grinding concentration is 68% ± 2%.
Citation Information
Patent Citations
Copper furnace slag mineral processing process
CN104399573A
Machine-column combined separation process suitable for fine-grain copper-nickel sulfide ore separation
CN115025884A