By employing high-frequency resistance welding and stress-relief annealing, the problem of welding cracks in cermet blades has been solved, enabling high-strength and high-efficiency production of cermet band saw blades and expanding their application scenarios.
Patent Information
- Application Number
- CN202410491993.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-23
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-04-23
AI Technical Summary
Metal-ceramic cutting tips are prone to welding cracks when using resistance welding, which limits their application in band saws.
High-frequency resistance welding is used to weld the metal-ceramic cutting head to the steel strip backing material, and stress-relief annealing is performed after welding. Combined with specific metal-ceramic formulations and coating treatments, welding parameters are controlled to ensure welding quality.
It improves the welding strength and durability of cermet band saw blades, overcomes the shortcomings of poor toughness of cermet, extends cutting life, and reduces production costs.
Smart Images

Figure CN118218683B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of band saw blade technology, specifically to a metal-ceramic band saw blade and its manufacturing method. Background Technology
[0002] Cermet is a heterogeneous composite material composed of a metal or alloy and one or more ceramic phases, combining some advantages of both metals and ceramics. Cermet (TiC(TiN)-WC+Ni(Mo)+Mo2C) used in cutting tools is a material with TiCN (ceramic) as the matrix (sometimes with the addition of other carbides and nitrides), and Ni, Mo, or Co (metal) as the binder (usually containing 10%–20% binder). Compared with traditional cemented carbide cutting tools, cermet cutting tools, in addition to high hardness and high wear resistance, have stable chemical properties, good oxidation resistance, and extremely low affinity between the material and the workpiece, making them less prone to tool sticking and built-up edge. They can achieve higher machining accuracy and good surface finish, and their hot hardness is higher than that of cemented carbide.
[0003] Table 1 Comparison of main components, advantages and disadvantages of cemented carbide and cermet.
[0004]
[0005] However, cermets have poor machinability (only grinding and EDM are possible), poor impact resistance, low strength and toughness, poor thermal conductivity, and are prone to hot cracking. Furthermore, the thermal expansion coefficients of cermets and steel differ significantly. Therefore, when cermets are used in tools with complex shapes and subjected to impact loads (such as circular saws), they are typically brazed in combination with steel. Brazing is a welding method that uses the thermodynamic properties of the brazing filler metal to weld the workpiece and filler metal together within a certain time and temperature range by heating the workpiece and filler metal. Brazing involves heating at relatively low temperatures and has a smaller thermal impact on the workpiece, but the weld strength is not high.
[0006] High-frequency resistance welding (HFRT) involves clamping the workpieces between two electrodes and heating them to melt the localized materials at the joint, bringing them to the necessary thermodynamic conditions for rapid bonding. Its advantages include fast welding speed, no need for brazing filler metal, low cost, and high weld strength. For welding band saw teeth, where the material needs to withstand significant impact, HFRT ensures better weld strength. Furthermore, cermets using HFRT can share welding production lines with carbide band saw blades, saving production costs. However, commercially available cermets are generally more brittle than carbide and have a significantly different coefficient of thermal expansion compared to steel. Resistance welding generates substantial thermal stress, leading industry professionals to generally believe that resistance welding of ordinary cermets is prone to hot cracking, which greatly limits their application in band saw teeth. Summary of the Invention
[0007] The purpose of this invention is to provide a metal-ceramic band saw blade and its manufacturing method, so as to solve the problem that metal-ceramic blades are prone to welding cracks when using resistance welding.
[0008] To achieve the above objectives, the present invention adopts the following technical solution:
[0009] A method for manufacturing a cermet band saw blade includes: welding a cermet cutting head to a steel strip backing material using high-frequency resistance welding, and then performing stress-relief annealing on the weld to obtain a cermet band saw blade.
[0010] In one preferred embodiment, the welding current is 800–1380 A and the welding time is 15–50 ms.
[0011] The purpose of welding is to weld the tooth material onto the backing material. This process requires melting the backing material, so the welding temperature must reach the melting temperature of the backing material. The welding current and time determine the temperature. The welding current and time must reach certain values to achieve the desired welding effect; otherwise, the welding strength will be insufficient. If the current is too high or the time is too long, firstly, the equipment has an upper limit, and secondly, the temperature will be too high, causing overheating, high thermal stress, and easy cracking of the metal ceramic.
[0012] In one preferred embodiment, the annealing temperature is 350–450°C.
[0013] Resistance welding is a common welding method that uses the heat effect generated by electric current to heat and join metals. Post-weld annealing is primarily to eliminate residual stress generated during welding, improve the microstructure of the weld area, and enhance the mechanical properties of the weld joint. During welding, the temperature undergoes rapid heating and cooling, thus stress concentration needs to be addressed. This helps reduce the likelihood of weld fracture during subsequent use. Too low a temperature will not achieve the desired stress relief. Excessively high annealing temperatures may have the following adverse effects on the welded workpiece:
[0014] 1. Grain growth: Excessively high annealing temperatures can lead to grain growth in the material, which reduces its strength and toughness. Coarse grains can also increase the brittleness of the material, thus affecting the overall performance of the welded joint.
[0015] 2. Deterioration of material properties: Excessive annealing temperature may affect the mechanical properties of the material and cause adverse changes in the microstructure, such as phase transformation or excessive softening.
[0016] 3. Heat-affected zone issues: During the welding process, the heat-affected zone may harden or overheat due to excessively high annealing temperatures, which increases the risk of cracks in the welded area.
[0017] 4. Oxidation and decarburization: At high temperatures, oxidation and decarburization are prone to occur on the surface of materials, which will reduce the surface quality and corrosion resistance of the materials.
[0018] 5. Thermal stress: Improper high-temperature annealing may cause new thermal stress inside the welded structure, which may lead to deformation or cracks in the welded structure.
[0019] 6. Delayed cracking: Some welding materials may develop delayed cracking after high-temperature annealing. This is because the diffusion and accumulation of hydrogen during high-temperature annealing may lead to embrittlement of the weld joint.
[0020] To ensure welding quality, annealing treatment requires precise control of annealing temperature and time based on the characteristics of the welding materials and the requirements of the welding process. Proper annealing can effectively eliminate residual welding stress, improve the performance of the welded joint, and extend the service life of the welded structure.
[0021] In one preferred embodiment, the steel strip backing material needs to undergo surface treatment before welding, and the surface treatment method is sandblasting.
[0022] The purpose of sandblasting is to clean the surface of the backing material, removing stains, oxidation, and individual burrs to facilitate welding.
[0023] In one preferred embodiment, the manufacturing method of the metal-ceramic band saw blade further includes: grinding the welded teeth, the welded area and the steel strip backing to remove the welding slag, and machining the required tooth shape and corresponding cutting edge on the teeth.
[0024] In one preferred embodiment, the grinding is performed using a resin-bonded diamond grinding wheel.
[0025] In one preferred embodiment, the method for manufacturing the metal-ceramic band saw blade further includes cleaning the band saw blade after grinding.
[0026] In one preferred embodiment, the cleaning step is as follows: sandblasting the band saw blade, cleaning it with compressed air and water to remove the grinding oil.
[0027] In one preferred embodiment, the steel strip backing material is prepared by forming and heat treatment.
[0028] In one preferred embodiment, the forming is performed by milling, grinding, laser cutting, water jet cutting, or wire cutting.
[0029] In one preferred embodiment, the heat treatment includes quenching and tempering. The quenching involves heating the steel strip backing material to 950°C to 1240°C in a vacuum or protective atmosphere, and then rapidly cooling it to room temperature in nitrogen or quenching oil. The material is then tempered 1 to 3 times at a tempering temperature of 450°C to 580°C.
[0030] In one preferred embodiment, the surface of the cermet tip needs to be plated with nickel or cobalt before welding.
[0031] The advantages of plating nickel or cobalt onto the surface of the cermet cutting tip before welding are:
[0032] 1. Improved corrosion resistance: The coating effectively prevents oxidation and corrosion of the weldment surface, especially in harsh environments such as those containing acids, alkalis, or other corrosive media. The coating forms a dense protective film that prevents corrosive media from contacting the base metal.
[0033] 2. Enhanced mechanical properties: The coating can improve the hardness and wear resistance of the weldment, reduce wear during the welding process, and thus extend the service life of the weldment. In particular, for this invention, the addition of the coating can significantly reduce the probability of welding cracks after resistance welding of metal ceramic cutting tips.
[0034] 3. Improved welding quality: The coating provides a smoother and more uniform surface, enhances the fluidity and wettability of the weld slag, and facilitates the uniform distribution of current during the welding process, thereby achieving better welding quality.
[0035] 4. Improve the conductivity of welded joints: Nickel and cobalt have good conductivity, and the coating can improve the conductivity of the weldment, which helps to effectively transfer current during resistance welding.
[0036] In one preferred embodiment, the coating thickness is 4–10 μm.
[0037] If the coating thickness is too small, the nickel (cobalt) plating will be insufficient; if the coating thickness is too large, the adhesion to the substrate will be poor, and the coating will easily peel off.
[0038] In one preferred embodiment, the coating thickness is 5–7 μm.
[0039] This coating range produces the best plating effect and the most stable welding.
[0040] In one preferred embodiment, the cermet tip has a density of 6.5–7.5 g / cm³, a hardness >90 HRA, and a fracture toughness ≥8 MPa. 1 / 2 Flexural strength ≥2000MPa, porosity A02B00, grain size 0.8~1.5μm.
[0041] Only when the performance of the cermet cutting tip is within a suitable range can we ensure successful welding and high-quality welds.
[0042] In one preferred embodiment, the cermet tip is made of TiC or Ti(C,N)-based cermet material, and its main components include: C 3%–4%, N 0–1%, Ti 35%–45%, V 0.3–0.6%, Co 9%–17%, Ni 4%–8%, Rb 0–4%, Nb 4–8%, Mo 0–4%, Ba 0–2%, Ta 5–10%, W 15%–20%, and Si 0–1%.
[0043] TiC or Ti(C,N)-based cermets are high-performance hard materials widely used in cutting tools, wear-resistant parts, and high-temperature applications. The roles of each component are as follows:
[0044] C (carbon): Carbon is the main component that forms TiC (titanium carbide). TiC has high hardness and wear resistance, and is a key component for improving the wear resistance of materials.
[0045] N (Nitrogen): The addition of nitrogen can form TiN (titanium nitride), which improves the hardness and corrosion resistance of the material, while also enhancing its thermal stability.
[0046] Ti (Titanium): Titanium is a constituent element of TiC and TiN, and is also one of the matrix components of cermets, which helps to improve the overall performance of the material.
[0047] Vanadium (V): Vanadium can improve the hardness and strength of materials, enhance wear resistance, and also help improve the thermal stability of materials.
[0048] Cobalt (Co): Cobalt is often used as a binder phase to improve the toughness and impact resistance of materials, and it also helps to improve the thermal conductivity of materials.
[0049] Ni (Ni): Nickel is also a binder phase, which helps to improve the toughness and corrosion resistance of materials, while also enhancing the thermal stability and oxidation resistance of materials.
[0050] Rb (rubidium): The addition of rubidium can improve the sintering properties of materials and help to increase the density and strength of materials.
[0051] Niobium (Nb): Niobium can improve the high-temperature strength and creep resistance of materials, and also helps to improve the toughness of materials.
[0052] Mo (Mo): The addition of molybdenum can improve the hardness and wear resistance of materials, and also help to improve the thermal stability and corrosion resistance of materials.
[0053] Ba (Barium): Barium may be used to improve the sintering properties and electrical conductivity of materials, but the specific role may vary depending on the material system.
[0054] Ta (tantalum): Tantalum can improve the high-temperature strength and creep resistance of materials, and also helps to improve the hardness and wear resistance of materials.
[0055] W (Tungsten): The addition of tungsten significantly improves the hardness and wear resistance of the material, while also enhancing its high-temperature performance and corrosion resistance.
[0056] Si (silicon): In cermets, silicon can improve strength and hardness, enhance wear resistance, and strengthen the oxidation resistance of materials.
[0057] The combination of these components gives TiC or Ti(C,N)-based cermets excellent overall properties, including high hardness, wear resistance, high temperature resistance and corrosion resistance, making them suitable for a variety of harsh working conditions.
[0058] However, not all TiC or Ti(C,N)-based cermets containing these elements are suitable for this invention.
[0059] The composition of cermet cutting tips is crucial for addressing the risk of welding cracks that may occur when using resistance welding with general cermet cutting tips. Not all cermet cutting tips are suitable. Through numerous experiments and explorations, this invention has concluded that cutting tip products that meet the requirements and satisfy subsequent welding can be prepared within the composition and range specified in this invention.
[0060] In one preferred embodiment, the main components of the cermet cutter tip include: C 3.2%–3.7%, N 0.5%–0.7%, Ti 38%–43%, V 0.4%–0.5%, Co 10%–16%, Ni 5%–7.5%, Rb 0–2.5%, Nb 5–7.5%, Mo 0–2.8%, Ba 1.5%–1.8%, Ta 5.5%–9.8%, W 17%–19.5%, and Si 0–0.8%.
[0061] After repeated experiments, it was found that the metal-ceramic cutting tip with this composition is less prone to cracking when using the resistance welding process of this invention.
[0062] In one preferred embodiment, the metal-ceramic particles in the metal-ceramic cutter head are prepared into cylindrical or spherical particles by sequentially ball milling, pressing, and sintering. The diameter φ of the cylindrical particles is 1.6-2.6 mm, and φ < L < φ + a, where L is the length of the cutter head and a ranges from 0.2 to 0.5 mm. The diameter of the spherical particles is 1.8-2.8 mm.
[0063] Only when the performance of the cermet cutting tip is within a suitable range can we ensure successful welding and high-quality welds.
[0064] This invention also claims protection for cermet band saw blades prepared according to the above-described preparation method.
[0065] High-frequency resistance welding is a welding method that uses the resistance heat generated by current passing through the contact surfaces of workpieces to achieve a metal-to-metal connection. For welding cermets and steel strips, the first consideration is the difference in their thermophysical properties, such as coefficients of thermal expansion, thermal conductivity, and melting points. Cermets typically have higher melting points and lower thermal conductivity, while steel strips have lower melting points and higher thermal conductivity. These differences necessitate precise control of temperature and heat distribution during welding to avoid damage to the materials. The welding process generally includes the following steps: 1. Pre-treatment: Before welding, the contact surfaces of the cermet and steel strip need to be cleaned to remove surface oxides, oil, and other contaminants to ensure good electrical contact and weld quality. 2. Pre-pressurization: Applying a certain pressure to ensure tight contact between the cermet and steel strip contact surfaces promotes current flow and heat transfer. 3. Electrical heating: Applying current to the workpiece through electrodes, according to Joule's law (Q = I0 / I0), the current is applied to the workpiece. 2 Rt), the resistance heat generated when the current passes through the contact surface will heat the contact area to a molten or plastic state. 4. Welding: During the heating process, the steel strip has a lower melting point and will melt before the ceramic material. At this time, the molten metal of the steel strip will fill the micropores and defects of the ceramic material, forming a bond between the metals. 5. Cooling: After welding, the welded area needs to be cooled slowly to avoid thermal stress and cracks caused by rapid cooling. 6. Post-processing: After welding, post-processing may be required, such as removing excess solder and repairing the weld, to ensure the quality and performance of the welded joint. When high-frequency resistance welding cermets and steel strips, special attention needs to be paid to controlling welding parameters, such as current magnitude, energizing time, pressure, etc., as well as the welding environment, such as temperature and atmosphere, to ensure the strength and durability of the welded joint. In addition, due to the high brittleness of cermets, excessive mechanical stress needs to be avoided during welding to prevent material fracture. To solve the technical problem of this invention, the present invention has discovered through multiple experiments that: 1. First, the toughness and porosity of the metal ceramic itself must meet the requirements; 2. The cutting tool must be plated with nickel or cobalt before welding; 3. Welding parameters, such as current and time, must be controlled and should not be too large.
[0066] This invention is the first to use high-frequency resistance welding as the welding method to weld metal ceramics and steel strip backing materials. By using a specific metal ceramic formula, selecting metal ceramic products that meet relevant performance requirements, and using appropriate coating types and thicknesses, metal ceramic tooth materials and steel strip backing materials can be welded under specific welding parameter conditions. This overcomes the problem that the thermal expansion coefficients of metal ceramics and steel are very different, and resistance welding would easily lead to welding cracks.
[0067] The beneficial effects of this invention are as follows:
[0068] 1. The cermet band saw blade prepared by this invention specifies the cermet tooth material formulation and process requirements suitable for the working conditions of cermet band saw blades. Compared with traditional carbide band saw blades, it fully utilizes the advantages of TiC or Ti(C,N) based cermets such as wear resistance, red hardness and oxidation resistance, resulting in a long cutting life, bright surface of the processed workpiece and good flatness. At the same time, it overcomes the disadvantage of poor toughness of cermets, thus expanding the application scenarios of cermet band saw blades.
[0069] 2. This invention uses high-frequency resistance welding to prepare metal-ceramic band saw blades. Compared with the brazing welding used in circular saws, it can effectively save costs and improve production efficiency. The prepared band saw blades have high welding strength and will not experience tooth breakage failure. Attached Figure Description
[0070] Figure 1 The metal-ceramic microstructure of Example 1;
[0071] Figure 2 These are nickel-plated metal-ceramic particles;
[0072] Figure 3 Comparison of wear on the teeth of carbide band saw blades and cermet band saw blades with the same number of cuts;
[0073] Left: Hard alloy; Right: Ceramic.
[0074] Figure 4 The metal-ceramic microstructure is shown in Comparative Example 2.
[0075] Figure 5 This is a photograph of the metal-ceramic welding crack in Comparative Example 3. Detailed Implementation
[0076] Comparative Example 1:
[0077] 1. Select carbide cutting tips with the following composition: WC 90%, Co 10%.
[0078] 2. The aforementioned cemented carbide cutting tips were sequentially processed through powder ball milling, pressing, and sintering to prepare cylindrical particles with a diameter φ = 2.2 mm and a length L = 2.5 mm. Testing revealed a density of 14.45 g / cm³, a hardness of 92.1 HRA, and a fracture toughness of 10.5 MPa. 1 / 2 It has a flexural strength of 3700MPa, a porosity of A02B00, and a grain size of 0.8~1μm.
[0079] 3. The surface of the carbide cutting tip is plated with nickel to a thickness of 5.5–6 μm.
[0080] Electroplating for nickel or electroless plating is a standard process that includes the following key steps:
[0081] Pretreatment includes passivation and pickling, the purpose of which is to make the workpiece surface smooth and clean, and increase adhesion;
[0082] Electroplating: Based on the desired nickel layer characteristics (such as bright nickel, high-sulfur nickel, nickel seal, etc.), prepare the appropriate electroplating solution, use the clean and activated base metal as the cathode and the nickel anode (pure nickel or sulfur-containing nickel) as the anode, and immerse them in the electroplating solution. By controlling the current and time, the nickel layer is deposited. The gloss, hardness and corrosion resistance of the nickel layer can be adjusted by changing the electroplating parameters (such as current density, temperature, pH value, etc.) and additives.
[0083] Electroless plating: The pre-treated cutting tool particles are immersed in an electroless plating solution containing nickel salts and corresponding additives. During this process, nickel ions are reduced to nickel and deposited on the surface of the cutting tool by a reducing agent (such as sodium hypophosphite).
[0084] Post-treatment: After electroplating or electroless plating is completed, the surface of the base metal needs to be washed with water and dried to prevent corrosion caused by moisture.
[0085] Additional post-processing steps, such as heat treatment or coating a protective layer, may be required as needed.
[0086] 4. The steel strip backing material is milled, heated to 1175℃ and quenched with quenching oil as the quenching medium, and then tempered three times at a tempering temperature of 550℃.
[0087] 5. After sandblasting the surface of the steel strip backing material, the carbide cutting tip is welded to the steel strip backing material using high-frequency resistance welding. The welding current is 1350A and the welding time is 25ms. After welding, the weld is subjected to stress-relief annealing at a temperature of 360℃.
[0088] 6. Grind the welded teeth, welded area, and steel strip backing material. Clean the band saw blade after grinding.
[0089] Example 1:
[0090] 1. Select a cermet tip with the following composition: C 3.4%, N 0.6%, Ti 38%, V 0.5%, Co 16%, Ni 5.3%, Nb 7.1%, Ba 1.5%, Ta 9.6%, W 18%.
[0091] 2. The above-mentioned cermet cutter heads were sequentially processed through powder ball milling, pressing, and sintering to prepare cylindrical particles with a diameter φ = 2.2 mm and a length L = 2.5 mm. Testing revealed a density of 7.3 g / cm³, a hardness of 91 HRA, and a fracture toughness of 9.5 MPa. 1 / 2 It has a flexural strength of 2450 MPa, a porosity of A02B00, and a grain size of 0.8–1 μm. (According to...) Figure 1 The metallographic structure of the ceramic was obtained.
[0092] 3. The surface of the metal-ceramic cutting tip is plated with nickel to a thickness of 5.5–6 μm, such as… Figure 2 As shown.
[0093] 4. The steel strip backing material is milled, heated to 1175℃ and quenched with quenching oil as the quenching medium, and then tempered three times at a tempering temperature of 550℃.
[0094] 5. After sandblasting the surface of the steel strip backing material, the metal ceramic cutter head is welded to the steel strip backing material using high-frequency resistance welding. The welding current is 1350A and the welding time is 25ms. After welding, the weld is subjected to stress-relief annealing at a temperature of 360℃.
[0095] 6. Grind the welded teeth, welded area, and steel strip backing material. Clean the band saw blade after grinding.
[0096] The band saw blades of Comparative Example 1 and Example 1 were compared, and the results are as follows: Figure 3 As shown, from Figure 3 It is evident that, when cutting the same material and with the same number of cuts (area), the wear resistance of cermet gears is significantly better than that of cemented carbide.
[0097] Comparative Example 2:
[0098] 1. Select a cermet tip with the following composition: C 3.6%, Ti 39%, V 0.5%, Co 11%, Ni 7.2%, Rb 2.4%, Nb 5.9%, Mo 2.7%, Ba 1.5%, Ta 6.6%, W 19%.
[0099] 2. The above-mentioned metal-ceramic cutting tips were sequentially processed through powder ball milling, pressing, and sintering to prepare cylindrical particles with a diameter of φ = 2.2 mm and a length of L = 2.5 mm. The density was measured to be 7.0 g / cm³. 3The hardness is 91.4 HRA, and the fracture toughness is 7 MPa.m. 1 / 2 The flexural strength is 1900 MPa, the porosity reaches A06B06, and the grain size is 1.5–2.0 μm (according to…). Figure 4 The metallographic structure of the metal-ceramic was obtained.
[0100] 3. The surface of the metal ceramic is plated with nickel to a thickness of 5.5–6 μm.
[0101] 4. The steel strip backing material is milled, heated to 1175℃ and quenched with quenching oil as the quenching medium, and then tempered three times at a tempering temperature of 550℃.
[0102] 5. After sandblasting the surface of the steel strip backing material, the metal ceramic cutter head is welded to the steel strip backing material using high-frequency resistance welding. The welding current is 1200A and the welding time is 25ms. After welding, the weld is subjected to stress-relief annealing at a temperature of 360℃.
[0103] 6. Because the fracture toughness, bending strength, porosity and grain size of the cutter head did not meet the requirements, the teeth cracked after welding.
[0104] This is because porosity and grain size have a significant impact on the mechanical properties of cermets, especially their toughness and crack resistance. 1. Pores, as internal defects, become sources of stress concentration when the material is subjected to external forces, increasing the risk of crack formation near the pores. 2. Pores reduce the load transfer efficiency within the material, resulting in uneven stress distribution and further increasing stress levels in localized areas. 3. Reduced overall strength: Pores reduce the actual load-bearing area of the material, thereby decreasing its overall strength and toughness. 4. Poor grain size usually indicates irregular atomic arrangement or defects at grain boundaries; these defects can become crack propagation paths, reducing the material's toughness. 5. If the grain size distribution is uneven, large grains may cause stress concentration in areas with smaller grains, increasing the likelihood of crack formation and propagation.
[0105] Therefore, if the porosity and grain size of the cermet do not meet the requirements, it will result in lower fracture toughness and bending strength, making it easier for stress concentration and crack propagation to occur during welding due to internal defects, leading to tooth cracking.
[0106] Example 2:
[0107] 1. Select a cermet tip with the following composition: C 3.5%, N 0.7%, Ti 42.9%, V 0.5%, Co 11%, Ni 7.6%, Rb 2.3%, Nb 5%, Mo 1.9%, Ba 1.8%, Ta 5.7%, W 17.1%.
[0108] 2. The above-mentioned cermet cutter heads were sequentially processed through powder ball milling, pressing, and sintering to prepare cylindrical particles with a diameter of φ = 2.5 mm and a length of L = 2.8 mm. Testing revealed a density of 6.96 g / cm³, a hardness of 91.8 HRA, and a fracture toughness of 8.8 MPa. 1 / 2 It has a flexural strength of 2200MPa, a porosity of A02B00, and a grain size of 1.0~1.3μm.
[0109] 3. The surface of the metal-ceramic cutter head is plated with cobalt at a depth of 7.0–7.5 μm.
[0110] 4. The steel strip backing material is milled, heated to 1150℃ and quenched with quenching oil as the quenching medium, and then tempered three times at a tempering temperature of 510℃.
[0111] 5. After sandblasting the surface of the steel strip backing material, the metal ceramic cutter head is welded to the steel strip backing material using high-frequency resistance welding. The welding current is 1180A and the welding time is 38ms. After welding, the weld is subjected to stress-relief annealing at a temperature of 400℃.
[0112] 6. Grind the welded teeth, welded area, and steel strip backing material. Clean the band saw blade after grinding.
[0113] Comparative Example 3:
[0114] 1. The same cutting tip with the same composition, size, and nickel plating standard as in Example 1, and the same steel strip backing material, but the cermet cutting tip has a fracture toughness of 7.6 MPa.m. 1 / 2 It has a bending strength of 1950MPa, a porosity of A04B04, a grain size of 1.5~1.8μm, and a surface nickel plating of 5.5~6μm.
[0115] 2. High-frequency resistance welding was performed on the cermet cutting head and steel strip backing material using a welding current of 1350A and a welding time of 25ms. After welding, the weld was subjected to stress-relief annealing at a temperature of 360℃. All other procedures were the same as in Example 1.
[0116] The results are as follows Figure 5 As shown, cracking occurred after the metal-ceramic welding. The reason may be that the fracture toughness, bending strength, porosity, and grain size of the cutting tip particles did not meet the requirements, resulting in cracking of the teeth after welding.
[0117] Comparative Example 4:
[0118] 1. Select a cermet tip with the following composition: C 8%, N 5%, Ti 48%, V 1%, Co 7%, Ni 3.5%, Nb 3.5%, Mo 7%, Ta 4%, W 13%.
[0119] 2. The above-mentioned cermet cutter head was sequentially processed through powder ball milling, pressing, and sintering to prepare cylindrical particles with a diameter of φ = 2.2 mm and a length of L = 2.5 mm. Testing revealed a density of 6.8 g / cm³ and a hardness of 92.1 HRA. Due to the low content of binders such as Co and Ni and the high content of hard phases such as TiC in the formulation, although this formulation could achieve higher hardness, its fracture toughness was only 7.5 MPa. 1 / 2 It has a bending strength of 1900MPa, is sintered, has a porosity of A02B02, a grain size of 0.8~1μm, and a nickel plating of 5.5~6μm on the cutter head surface.
[0120] 3. The cermet cutting tip and the steel strip backing were welded using high-frequency resistance welding. Four sets of welding parameters were tested: welding current 900A, welding time 18ms; welding current 1360A, welding time 40ms; welding current 1350A, welding time 25ms; welding current 1180A, welding time 38ms. After welding, the weld was subjected to stress-relief annealing at a temperature of 380℃.
[0121] The unsuitable composition range of the metal-ceramic formula for the cutting head, such as low content of binders like Co and Ni and excessive content of hard phases like TiC, resulted in the failure of the prepared particles to meet the requirements for fracture toughness, bending strength, and porosity. Consequently, tooth cracking occurred after welding with different welding parameters.
[0122] Comparative Example 5:
[0123] 1. The same cutting head with the same composition, size, and performance standards as in Example 2, and the same steel strip backing material, but with a cobalt plating of only 1.5μm.
[0124] 2. The cermet cutting tip was welded to the steel strip backing material using high-frequency resistance welding at a current of 1450A for 26ms. After welding, the weld was subjected to stress-relief annealing at 400℃. At this temperature, the weld strength was lower than the standard value, and the welded teeth exhibited significant embrittlement, with fracture toughness decreasing to only 5MPa. . m 1 / 2 .
[0125] Comparative Example 6:
[0126] 1. Use the same cutting tip with the same composition, size, performance and nickel plating standard as in Example 1, and the same steel strip backing material.
[0127] 2. The cermet cutting tip and the steel strip backing material were welded using high-frequency resistance welding. The welding current was adjusted to 1350A and the welding time was 10ms, while other parameters remained unchanged. At this time, the welding strength was lower than the standard value. The welding current was kept unchanged, and the welding time was adjusted to 60ms, while other parameters remained unchanged. At this time, the welding strength was higher than the standard value, but some cracks and overheating oxidation were present in the teeth.
[0128] Comparative Example 7:
[0129] 1. Use the same cutting tip with the same composition, size, performance and nickel plating standard as in Example 1, and the same steel strip backing material.
[0130] 2. The cermet cutting tip and the steel strip backing were welded using high-frequency resistance welding. The welding time was 25ms, and the welding current was adjusted to 750A while keeping other parameters unchanged. At this time, the welding strength was lower than the standard value. When the welding current was adjusted to 1400A while keeping other parameters unchanged, the welding strength was higher than the standard value, but there was some cracking and overheating oxidation in the teeth.
Claims
1. A method for manufacturing a metal-ceramic band saw blade, characterized in that, include: The metal-ceramic cutting head is welded to the steel strip backing material using high-frequency resistance welding. After welding, the weld is subjected to stress-relief annealing to obtain a metal-ceramic band saw blade. The cermet cutting tip is made of TiC or Ti(C,N) based cermet material, and its main components include: C 3%~4%, N 0~1%, Ti 35%~45%, V 0.3~0.6%, Co 9%~17%, Ni 4%~8%, Rb 0~4%, Nb 4~8%, Mo 0~4%, Ba 0~2%, Ta 5~10%, W 15%~20%, and Si 0~1%.
2. The manufacturing method according to claim 1, characterized in that, The welding current is 800~1380A, and the welding time is 15~50ms.
3. The manufacturing method according to claim 1, characterized in that, The stress-relief annealing temperature is 350~450℃.
4. The manufacturing method according to claim 1, characterized in that, The manufacturing method of the metal-ceramic band saw blade further includes: grinding the welded teeth, the welded area and the steel strip backing to remove the welding slag, and machining the required tooth shape and corresponding cutting edge on the teeth.
5. The manufacturing method according to claim 1, characterized in that, Before welding, the surface of the metal-ceramic cutting tip needs to be plated with nickel or cobalt.
6. The manufacturing method according to claim 5, characterized in that, The coating thickness is 4~10μm.
7. The manufacturing method according to claim 1, characterized in that, The density of the cermet cutting tip is 6.5~7.5 g / cm³, the hardness is >90 HRA, and the fracture toughness is ≥8 MPa·m. 1 / 2 The flexural strength is ≥2000MPa, the porosity reaches A02B00, and the grain size is 0.8~1.5μm.
8. The manufacturing method according to claim 1, characterized in that, The cermet particles in the cermet cutter head are prepared into cylindrical or spherical particles by sequentially ball milling, pressing, and sintering. The diameter φ of the cylindrical particles is 1.6-2.6 mm, and φ < L < φ + a, where L is the length of the cutter head and a ranges from 0.2 to 0.5 mm. The diameter of the spherical particles is 1.8-2.8 mm.
9. A metal-ceramic band saw blade prepared by the manufacturing method according to any one of claims 1-8.
Citation Information
Patent Citations
Tip bonding method and saw blade
JP2016144835A