Hydrogen bond enhanced graphene composite shape memory polymer and preparation method and application thereof
By using hydrogen-bonded graphene composite materials, combined with covalent modification of graphene oxide and a strong hydrogen bond donor of "pyridine + ketone", a high-strength and tough shape memory polymer was prepared. This solved the problems of microstructure changes and crack propagation in shape memory polymers during friction, and achieved a balance between high mechanical properties and self-healing ability.
Patent Information
- Application Number
- CN202410329898.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-22
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-03-22
AI Technical Summary
Existing shape memory polymers cannot effectively address the microstructure changes and crack propagation caused by interfacial material energy exchange during friction, making it difficult to achieve a balance between high mechanical properties and self-healing capabilities.
By introducing hydrogen-bonded graphene composite materials, utilizing covalent modification of graphene oxide surface and strong hydrogen bond donors of "pyridine + ketone", combined with the reinforcement of two-dimensional nanofillers and the toughening mechanism of sacrificial bonds, a high-strength and tough shape memory PI-PUU block copolymer was prepared.
It achieves a balance between high mechanical properties and self-healing ability, improving the material's shape memory properties, self-healing ability, and wear resistance.
Smart Images

Figure CN118222101B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of shape memory materials technology, specifically to a hydrogen bond-enhanced graphene composite shape memory polymer, its preparation method, and its applications. Background Technology
[0002] Polymer materials inevitably develop micro or macro cracks during service due to friction, wear, thermal fatigue, and mechanical fatigue, which affects their usability. Designing and developing self-healing smart supramolecular materials, mimicking natural flora and fauna, for applications in functional coatings, wearable electronic devices, soft robots, electronic skin, and artificial muscles can significantly extend service life and durability. However, achieving a balance between high mechanical strength and good self-healing capabilities remains a challenge.
[0003] Shape memory polymers (SMPs) possess unique stimulus-response properties, integrating polymer and actuation characteristics. Relying on their structural and thermodynamic properties, SMPs can convert thermal energy into kinetic energy, thereby achieving actuation. However, this shape recovery cannot fundamentally address the microscopic morphological changes (e.g., extrusion deformation, mass loss, crack propagation) and sealing performance loss caused by interfacial energy exchange during friction. Therefore, to overturn traditional thinking, utilizing molecular structure design methods to improve the strength and toughness of shape memory polymers has significant theoretical and practical application implications. Currently, the most effective strategy for synthesizing tough self-healing materials is through non-covalent / covalent interactions as sacrificial bonds and reversible crosslinking. Guan et al. (Y. Chen, A.M. Kushner, G.A. Williams, Z. Guan, Multiphase design of autonomic self-healing thermoplastic elastomers. Nature Chem. 2012, 4(6), 467-472.) synthesized a multiphase supramolecular material with high toughness and self-healing ability using non-covalent interactions as sacrificial bonds. Bao (X.Yan,Z.Liu,Q.Zhang,J.Lopez,H.Wang,H.-C.Wu,S.Niu,H.Yan,S.Wang,T.Lei,J.Li,D.Qi,P.Huang,J.Huang,Y.Zhang,Y.Wang,G.Li,JBHTok,X.Chen,Z.Bao,Quadruple H-Bonding Cross-Linked Supramolecular Polymeric Materials as Substrates for Stretchable, Antititearing, and Self-Healable ThinFilm Electrodes.J.Am.Chem.Soc.2018,140(15),5280-5289.) synthesized a self-healing supramolecular elastic material with excellent tensile properties based on a strongly reversible quadruple hydrogen-bonded crosslinking agent. However, maintaining the self-healing ability of the material while achieving high mechanical properties remains a key challenge. Summary of the Invention
[0004] The purpose of this invention is to provide a hydrogen bond-enhanced graphene composite shape memory polymer, its preparation method, and its application. The hydrogen bond-enhanced graphene composite shape memory polymer prepared by this invention has excellent shape memory properties, self-healing properties, wear resistance, and other comprehensive properties.
[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solution:
[0006] This invention provides a method for preparing a hydrogen-bonded reinforced graphene composite shape memory polymer, comprising the following steps:
[0007] Diisocyanate, diol and first catalyst are mixed and subjected to first polymerization reaction to obtain polyurethane prepolymer;
[0008] The polyurethane prepolymer, bifunctional aminobiphenyl and diacid dihydrazide monomers are mixed and subjected to a second polymerization reaction to obtain amino-terminated PUU molecular chains.
[0009] 4,4'-diisocyanate-3,3'-dimethylbiphenyl, acid anhydride and second catalyst were mixed and subjected to a third polymerization reaction to obtain isocyanate-terminated PI molecular chains.
[0010] The amino-terminated PUU molecular chains and isocyanate-terminated PI molecular chains are mixed and subjected to a fourth polymerization reaction to obtain a shape memory PI-PUU block copolymer.
[0011] Graphene oxide, 3-(aminomethyl)-4,6-dimethylpyridine-2(1H)-one, a first organic solvent and a third catalyst were mixed and grafted to obtain graphene oxide covalently modified with 3-(aminomethyl)-4,6-dimethylpyridine-2(1H)-one.
[0012] The shape memory PI-PUU block copolymer, 3-(aminomethyl)-4,6-dimethylpyridine-2(1H)-one covalently modified graphene oxide, and a second organic solvent were mixed and cured to obtain a hydrogen bond-enhanced graphene composite shape memory polymer.
[0013] Preferably, the diisocyanate includes one or more of isophorone diisocyanate, 1,6-hexane diisocyanate, terephthalic diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate and phenyldimethyl diisocyanate.
[0014] The diol includes one or more of polycarbonate diol and polytetramethylene ether diol;
[0015] The first catalyst comprises dibutyltin dilaurate or stannous octoate;
[0016] The molar ratio of the diisocyanate to the diol is 2:1; the mass of the first catalyst is 0.01 to 0.03 wt% of the total mass of the diisocyanate and the diol.
[0017] The temperature of the first polymerization reaction is 70–100°C; the time of the first polymerization reaction is 2–4 hours.
[0018] Preferably, the bifunctional aminobiphenyl comprises one or more of 2,2'-bis(trifluoromethyl)diaminobiphenyl, 3,3'-dichloro-4,4'-diaminodiphenylmethane, 3,5-diamino-p-chlorobenzoate isobutyl ester, and diethyltoluenediamine.
[0019] The diacylhydrazine monomer includes one or more of adipic diacylhydrazine, oxalic diacylhydrazine, malonic diacylhydrazine, succinic diacylhydrazine, azelaic diacylhydrazine, and dodecanedicarboxylic diacylhydrazine;
[0020] The molar ratio of the diisocyanate to the difunctional aminobiphenyl is 10:0.1-3; the molar ratio of the diisocyanate to the diacylhydrazine monomer is 10:2.6-5.6.
[0021] The temperature of the second polymerization reaction is 70–100°C; the time of the second polymerization reaction is 6–12 hours.
[0022] Preferably, the acid anhydride includes one or more of 4,4'-(hexafluoroisopropene) phthalic anhydride, benzophenone dianhydride, pyromellitic dianhydride, diphenyl ether dianhydride, and biphenyl dianhydride;
[0023] The second catalyst comprises N,N-dimethylcyclohexylamine and N-methylaniline; the mass ratio of N,N-dimethylcyclohexylamine to N-methylaniline is 2:1 to 3;
[0024] The molar ratio of 4,4'-diisocyanate-3,3'-dimethylbiphenyl to acid anhydride is 1 to 2:1; the mass of the second catalyst is 0.01 to 0.03 wt% of the total mass of 4,4'-diisocyanate-3,3'-dimethylbiphenyl and acid anhydride.
[0025] The temperature of the third polymerization reaction is 130–160°C; the time of the third polymerization reaction is 10–24 hours.
[0026] Preferably, the temperature of the fourth polymerization reaction is 60–100°C; and the time of the fourth polymerization reaction is 24–60 hours.
[0027] Preferably, the first organic solvent includes N,N-dimethylformamide or N,N-dimethylacetamide;
[0028] The third catalyst comprises 4-dimethylaminopyridine and N,N'-dicyclohexylcarbodiimide; the mass ratio of 4-dimethylaminopyridine to N,N'-dicyclohexylcarbodiimide is 2:1 to 3.
[0029] The mass ratio of the graphene oxide to 3-(aminomethyl)-4,6-dimethylpyridin-2(1H)-one is 0.06:0.04 to 0.06;
[0030] The mass ratio of graphene oxide to the third catalyst is 100:0.01 to 0.03.
[0031] Preferably, the grafting reaction temperature is 0–25°C; and the grafting reaction time is 24–48 hours.
[0032] Preferably, the second organic solvent includes N,N-dimethylformamide or N,N-dimethylacetamide;
[0033] The mass ratio of the shape memory PI-PUU block copolymer and the 3-(aminomethyl)-4,6-dimethylpyridine-2(1H)-one covalently modified graphene oxide is 100:0.1-2.
[0034] The present invention provides a hydrogen bond-enhanced graphene composite shape memory polymer prepared by the preparation method described above, comprising a shape memory PI-PUU block copolymer and 3-(aminomethyl)-4,6-dimethylpyridine-2(1H)-one covalently modified graphene oxide added to the shape memory PI-PUU block copolymer.
[0035] This invention provides the application of the hydrogen bond-enhanced graphene composite shape memory polymer described above in the preparation of functional coatings, wearable electronic devices, soft robots, electronic skin, or artificial muscles.
[0036] This invention provides a method for preparing hydrogen bond-enhanced graphene composite shape memory polymers. This invention utilizes a hydrogen bond enhancement strategy for graphene oxide to covalently modify the surface of graphene oxide, introducing a strong hydrogen bond donor of "pyridine + ketone". By combining the two-dimensional nanofiller reinforcement with the sacrificial bond toughening mechanism, this invention achieves the successful preparation of high-strength and tough shape memory PI-PUU block copolymers. Attached Figure Description
[0037] Figure 1 This is a schematic diagram of the structure of the hydrogen bond-enhanced graphene composite shape memory polymer prepared in this invention. Detailed Implementation
[0038] This invention provides a method for preparing a hydrogen-bonded reinforced graphene composite shape memory polymer, comprising the following steps:
[0039] Diisocyanate, diol and first catalyst are mixed and subjected to first polymerization reaction to obtain polyurethane prepolymer;
[0040] The polyurethane prepolymer, bifunctional aminobiphenyl and diacid dihydrazide monomers are mixed and subjected to a second polymerization reaction to obtain amino-terminated PUU molecular chains.
[0041] 4,4'-diisocyanate-3,3'-dimethylbiphenyl, acid anhydride and second catalyst were mixed and subjected to a third polymerization reaction to obtain isocyanate-terminated PI molecular chains.
[0042] The amino-terminated PUU molecular chains and isocyanate-terminated PI molecular chains are mixed and subjected to a fourth polymerization reaction to obtain a shape memory PI-PUU block copolymer.
[0043] Graphene oxide, 3-(aminomethyl)-4,6-dimethylpyridine-2(1H)-one, a first organic solvent and a third catalyst were mixed and grafted to obtain graphene oxide covalently modified with 3-(aminomethyl)-4,6-dimethylpyridine-2(1H)-one.
[0044] The shape memory PI-PUU block copolymer, 3-(aminomethyl)-4,6-dimethylpyridine-2(1H)-one covalently modified graphene oxide, and a second organic solvent were mixed and cured to obtain a hydrogen bond-enhanced graphene composite shape memory polymer.
[0045] In this invention, diisocyanate, diol and a first catalyst are mixed to carry out a first polymerization reaction to obtain a polyurethane prepolymer.
[0046] In this invention, the diisocyanate preferably includes one or more of isophorone diisocyanate (IPDI), 1,6-hexanediisocyanate, terephthalic diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, and phenylenediamine diisocyanate; the diol preferably includes one or more of polycarbonate diol (PCDL) and polytetramethylene ether diol; the first catalyst preferably includes dibutyltin dilaurate (DBTDL) or stannous octoate. In this invention, the number average molecular weight of the diol is preferably 1000-5000, more preferably 2000. In this invention, the diol is preferably dehydrated before use. In this invention, the molar ratio of the diisocyanate to the diol is preferably 2:1; the mass of the first catalyst is preferably 0.01-0.03 wt% of the total mass of the diisocyanate and the diol, more preferably 0.01 wt%.
[0047] In this invention, the temperature of the first polymerization reaction is preferably 70–100°C, more preferably 80–90°C; the time of the first polymerization reaction is preferably 2–4 hours, more preferably 2.5–3 hours. In this invention, the atmosphere of the first polymerization reaction is preferably a nitrogen atmosphere.
[0048] After obtaining the polyurethane prepolymer, the present invention mixes the polyurethane prepolymer, the bifunctional aminobiphenyl and the diacid dihydrazide monomer, and carries out a second polymerization reaction to obtain amino-terminated PUU molecular chains.
[0049] In this invention, the difunctional aminobiphenyl preferably comprises one or more of 2,2'-bis(trifluoromethyl)diaminobiphenyl, 3,3'-dichloro-4,4'-diaminodiphenylmethane, 3,5-diamino-p-chlorobenzoate isobutyl ester, and diethyltoluenediamine. In this invention, the diacid hydrazide monomer preferably comprises one or more of adipate diacid hydrazide (ADH), oxalate diacid hydrazide, malonate diacid hydrazide, succinate diacid hydrazide, azelaic acid diacid hydrazide, and dodecanedicarboxylic acid diacid hydrazide. In this invention, the molar ratio of the diisocyanate to the difunctional aminobiphenyl is preferably 10:0.1–3, more preferably 10:0.1–2.4; the molar ratio of the diisocyanate to the diacid hydrazide monomer is preferably 10:2.6–5.6, more preferably 10:3.1–5.6.
[0050] In this invention, the temperature of the second polymerization reaction is preferably 70–100°C, more preferably 80–90°C; the time of the second polymerization reaction is preferably 6–12 hours, more preferably 12 hours. In this invention, the second polymerization reaction is preferably carried out under oil bath conditions. In this invention, the atmosphere of the second polymerization reaction is preferably a nitrogen atmosphere.
[0051] In this invention, 4,4'-diisocyanate-3,3'-dimethylbiphenyl (TODI), an anhydride, and a second catalyst are mixed and subjected to a third polymerization reaction to obtain isocyanate-terminated PI molecular chains.
[0052] In this invention, the anhydride preferably includes one or more of 4,4'-(hexafluoroisopropene)phthalic anhydride (6FDA), benzophenone dianhydride, pyromellitic dianhydride, diphenyl ether dianhydride, and biphenyl dianhydride; the second catalyst includes N,N-dimethylcyclohexylamine (DMCA) and N-methylaniline (NMA); the mass ratio of N,N-dimethylcyclohexylamine to N-methylaniline is preferably 2:1 to 3, more preferably 2:1.
[0053] In this invention, the molar ratio of 4,4'-diisocyanate-3,3'-dimethylbiphenyl and acid anhydride is preferably 1 to 2:1, more preferably 1.1:1; the mass of the second catalyst is preferably 0.01 to 0.03 wt% of the total mass of 4,4'-diisocyanate-3,3'-dimethylbiphenyl and acid anhydride, more preferably 0.01 wt%.
[0054] In this invention, the mixing of 4,4'-diisocyanate-3,3'-dimethylbiphenyl (TODI), the acid anhydride, and the second catalyst preferably comprises: first heating and stirring 4,4'-diisocyanate-3,3'-dimethylbiphenyl (TODI) and the acid anhydride, and then adding the second catalyst. In this invention, the heating and stirring temperature is preferably 100–130°C, more preferably 110–120°C; the heating and stirring time is preferably 5–20 min, more preferably 10–15 min. In this invention, the mixing is preferably carried out under a nitrogen atmosphere.
[0055] In this invention, the temperature of the third polymerization reaction is preferably 130–160°C, more preferably 140–150°C; the time of the third polymerization reaction is preferably 10–24 hours, more preferably 12–20 hours. In this invention, the atmosphere of the third polymerization reaction is preferably a nitrogen atmosphere.
[0056] After obtaining amino-terminated PUU molecular chains and isocyanate-terminated PI molecular chains, the present invention mixes the amino-terminated PUU molecular chains and isocyanate-terminated PI molecular chains and carries out a fourth polymerization reaction to obtain shape memory PI-PUU block copolymers.
[0057] In this invention, the temperature of the fourth polymerization reaction is preferably 60–100°C, more preferably 80–90°C; the time of the fourth polymerization reaction is preferably 24–60 hours, more preferably 30–48 hours. In this invention, the atmosphere of the fourth polymerization reaction is preferably a nitrogen atmosphere.
[0058] In a specific embodiment of the present invention, after the second and third polymerization reactions are completed, the reaction system containing amino-terminated PUU molecular chains and the reaction system containing isocyanate-terminated PI molecular chains are directly mixed to carry out a fourth polymerization reaction to obtain a shape memory PI-PUU block copolymer.
[0059] Following the fourth polymerization reaction, the present invention preferably includes removing the solvent from the system to obtain a shape memory PI-PUU block copolymer. In the present invention, the method for removing the solvent from the system preferably includes drying at 80°C.
[0060] In this invention, the PI content of the shape memory PI-PUU block copolymer is preferably 20-24 wt%, more preferably 23.2 wt%.
[0061] In specific embodiments of the present invention, no separation or purification is performed during the preparation of the shape memory PI-PUU block copolymer.
[0062] In this invention, graphene oxide, 3-(aminomethyl)-4,6-dimethylpyridin-2(1H)-one, a first organic solvent and a third catalyst are mixed and grafted to obtain graphene oxide covalently modified with 3-(aminomethyl)-4,6-dimethylpyridin-2(1H)-one.
[0063] In this invention, the first organic solvent preferably includes N,N-dimethylformamide (DMF) or N,N-dimethylacetamide; the third catalyst preferably includes 4-dimethylaminopyridine and N,N'-dicyclohexylcarbodiimide; the mass ratio of 4-dimethylaminopyridine to N,N'-dicyclohexylcarbodiimide is preferably 2:1 to 3, more preferably 2:1.
[0064] In this invention, the mass ratio of graphene oxide to 3-(aminomethyl)-4,6-dimethylpyridin-2(1H)-one is preferably 0.06:0.04 to 0.06, more preferably 0.06:0.05. In this invention, the mass ratio of graphene oxide to the third catalyst is preferably 100:0.01 to 0.03, more preferably 100:0.02. This invention does not have special requirements on the amount of the first solvent, as long as it is sufficient to uniformly disperse the graphene oxide.
[0065] In this invention, the temperature of the grafting reaction is preferably 0–25°C, more preferably 0°C; the time of the grafting reaction is preferably 24–48 hours, more preferably 24 hours. In this invention, the atmosphere of the grafting reaction is preferably atmospheric.
[0066] Following the grafting reaction, the present invention preferably further includes: centrifuging and washing the resulting reaction system, dispersing the resulting product in water, and freeze-drying to obtain 3-(aminomethyl)-4,6-dimethylpyridin-2(1H)-one covalently modified graphene oxide. In this invention, the washing solution used for centrifugation and washing is preferably water; the number of centrifugation and washing cycles is preferably 3. In this invention, the freeze-drying temperature is preferably -50°C; the freeze-drying time is preferably 48 hours.
[0067] After obtaining the shape memory PI-PUU block copolymer and the 3-(aminomethyl)-4,6-dimethylpyridine-2(1H)-one covalently modified graphene oxide, the present invention mixes the shape memory PI-PUU block copolymer, the 3-(aminomethyl)-4,6-dimethylpyridine-2(1H)-one covalently modified graphene oxide and a second organic solvent, and after curing, obtains a hydrogen bond-enhanced graphene composite shape memory polymer.
[0068] In this invention, the second organic solvent preferably includes N,N-dimethylformamide or N,N-dimethylacetamide. In this invention, the mass ratio of the shape memory PI-PUU block copolymer to the 3-(aminomethyl)-4,6-dimethylpyridin-2(1H)-one covalently modified graphene oxide is preferably 100:0.1–2, more preferably 100:0.25–1. This invention does not have special requirements on the amount of the second organic solvent, as long as it is sufficient to dissolve the shape memory PI-PUU block copolymer.
[0069] In this invention, the curing method preferably includes drying; the drying temperature is preferably 80°C.
[0070] The present invention also provides a hydrogen bond-enhanced graphene composite shape memory polymer prepared by the preparation method described above, comprising a shape memory PI-PUU block copolymer and 3-(aminomethyl)-4,6-dimethylpyridine-2(1H)-one covalently modified graphene oxide added to the shape memory PI-PUU block copolymer.
[0071] Figure 1 This is a schematic diagram of the structure of the hydrogen bond-enhanced graphene composite shape memory polymer prepared according to the present invention. From the perspective of molecular design, the present invention introduces multiple hydrogen bonds in the process of soft (PUU) / hard (PI) segment block design to comprehensively improve the strength and toughness of the material. From the perspective of filler design, strong hydrogen bond acceptors (pyridine + ketone) are modified on the surface of graphene oxide to enhance the dynamic binding ability of filler and polymer molecular chain segments, further improving the comprehensive properties of the material, including shape memory, self-healing, wear resistance, etc.
[0072] This invention also provides the application of the hydrogen bond-enhanced graphene composite shape memory polymer described above in the preparation of functional coatings, wearable electronic devices, soft robots, electronic skin, or artificial muscles.
[0073] The technical solutions of this invention will be clearly and completely described below with reference to the embodiments thereof. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0074] The raw materials used in the examples and comparative examples are shown in Table 1:
[0075] Table 1. Raw materials used in the examples and comparative examples.
[0076]
[0077] Example 1
[0078] 1. Shape memory PI-PUU block copolymer:
[0079] (1) Add 10 mmol IPDI to 5 mmol PCDL and add 0.01 wt% DBTDL as a catalyst, and react for 2.5 hours in an oil bath at 80 °C under nitrogen protection.
[0080] (2) 3.1 mmol ADH and 2.4 mmol TFDB were added to the above solution one after another, and the reaction was continued at 80 °C for 10 hours to obtain a reaction system containing amino-terminated PUU molecular chains;
[0081] (3) 5.4 mmol 6FDA was added to 6 mmol TODI under nitrogen protection. After stirring at 120°C for 10 minutes, 0.01 wt% DMCA and NMA (DMCA and NMA in a mass ratio of 2:1) were added as catalysts. The temperature was then raised to 150°C and the reaction was carried out for 12 hours to obtain a reaction system containing PI molecular chains with isocyanate end caps.
[0082] (4) The reaction system containing amino-terminated PUU molecular chains is blended with the reaction system containing isocyanate-terminated PI molecular chains, and the mixture is reacted for 48 hours in an oil bath at 90°C under nitrogen protection. After removing the solvent at 80°C, the shape memory PI-PUU block copolymer is obtained and named AFF.
[0083] 2. Preparation of MG
[0084] 0.06 g of GO was ultrasonically dispersed in 60 mL of DMF, and 0.05 g of MDO was added. Subsequently, 0.01 wt% of DMAP and DCC (the mass ratio of DMAP to DCC was 2:1) were added, and the reaction was carried out at 0 °C under atmospheric atmosphere for 24 hours. The product was centrifuged and washed three times (washing solution was water), and then dispersed in water. The product was freeze-dried at -50 °C for 48 hours to obtain 3-(aminomethyl)-4,6-dimethylpyridin-2(1H)-one covalently modified graphene oxide, named MG.
[0085] 3. Preparation of hydrogen bond-enhanced graphene composite shape memory polymers
[0086] 10g of the shape memory PI-PUU block copolymer was dissolved in 20mL of DMF, 0.025g of the MG was added, and the mixture was stirred evenly and then cured in an oven at 80℃ to obtain a hydrogen bond-enhanced graphene composite shape memory polymer, named AFF@MG-0.25wt.%.
[0087] Example 2
[0088] The preparation process of shape memory PI-PUU block copolymer and MG is the same as in Example 1;
[0089] 10g of the shape memory PI-PUU block copolymer was dissolved in 20mL of DMF, 0.05g of the MG was added, and the mixture was stirred evenly and then cured in an oven at 80℃. The resulting hydrogen bond-reinforced graphene composite shape memory polymer was named AFF@MG-0.5wt.%.
[0090] Example 3
[0091] The preparation process of shape memory PI-PUU block copolymer and MG is the same as in Example 1;
[0092] 10g of the shape memory PI-PUU block copolymer was dissolved in 20mL of DMF, 0.1g of the MG was added, and the mixture was stirred evenly and then cured in an oven at 80℃. The resulting hydrogen bond-enhanced graphene composite shape memory polymer was named AFF@MG-1wt.%.
[0093] Comparative Example 1
[0094] (1) Add 10 mmol IPDI to 5 mmol PCDL and add 0.01 wt% DBTDL as a catalyst, and react for 2.5 hours in an oil bath at 80 °C under nitrogen protection.
[0095] (2) Add 5.6 mmol ADH to the above solution and continue the reaction at 80 °C for 10 hours to obtain a reaction system containing an amino-terminated PUU segment;
[0096] (3) 5.4 mmol 6FDA was added to 6 mmol TODI under nitrogen protection. After stirring at 120°C for 10 minutes, 0.01 wt% DMCA and NMA (DMCA and NMA in a mass ratio of 2:1) were added as catalysts. The temperature was then raised to 150°C and the reaction was carried out for 12 hours to obtain a reaction system containing isocyanate-terminated PI molecular chains.
[0097] (4) The reaction system containing amino-terminated PUU segments is blended with the reaction system containing isocyanate-terminated PI molecular chains, and the reaction is carried out in an oil bath at 90°C and under nitrogen protection for 48 hours. After solvent removal at 80°C, PI-PUU block copolymer is obtained and named AFF-1.
[0098] Comparative Example 2
[0099] The preparation process of the shape memory PI-PUU block copolymer is the same as in Example 1;
[0100] 10g of the shape memory PI-PUU block copolymer was dissolved in 20mL of DMF, 0.05g of GO was added, and the mixture was stirred evenly and then cured in an oven at 80℃. The resulting shape memory polymer was named AFF@GO-0.5wt.%.
[0101] Test case
[0102] Table 2 shows the performance comparison of Examples 1-3 and Comparative Examples 1-2. The test standards for fracture strength and elongation at break are GB / T 1040.1-2018, the test standards for friction coefficient and wear rate are GB / T3960-1983, and the test standard for glass transition temperature is GB / T 36800.2-2018.
[0103] The method for detecting shape fixation rate and shape recovery rate is as follows: (i) heat the sample at a rate of 5K / min to T g (ii) Hold at +30℃ for 5 minutes, then apply a stable force to the sample for tensile testing; (ii) Hold the force and cool to 90℃ at a rate of 5 K / min, and hold at 90℃ for 5 minutes. The strain at this point is denoted as ε. load (iii) Next, unload the external force to obtain ε. unload (iv) To verify the shape recovery properties of the SMP, the temperature was reheated to T at a rate of 5 K / min. g +30℃, and at T g The sample was held at +30℃ for 20 minutes. During the heating process, the force was unloaded, and the sample was in an unloaded state. The final strain is denoted as ε. rec (The deformation temperature and the shape-fixing temperature are respectively selected as T.) g +30℃ and 90℃, with heating and cooling rates both set to 5K / min. Where N represents the number of shape memory cycles.
[0104] Shape fixation rate (R) f ) and shape recovery rate (R r The calculation formula for ) is as follows:
[0105]
[0106]
[0107] Table 2 Performance comparison of Examples 1-3 and Comparative Examples 1-2
[0108]
[0109] As shown in Table 2, the hydrogen-bonded reinforced graphene composite shape memory polymer (AFF@MG) prepared in this invention exhibits good strength and toughness, achieving a combination of strength and toughness. Furthermore, with the increase of MG content in the PI-PUU block shape memory copolymer, the fracture strength of the sample increases, while the elongation at break decreases.
[0110] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a hydrogen bond-enhanced graphene composite shape memory polymer, comprising the following steps: Diisocyanate, diol and first catalyst are mixed and subjected to first polymerization reaction to obtain polyurethane prepolymer; The polyurethane prepolymer, bifunctional aminobiphenyl and diacid dihydrazide monomer are mixed and subjected to a second polymerization reaction to obtain amino-terminated PUU molecular chains; the bifunctional aminobiphenyl is 2,2'-bis(trifluoromethyl)diaminobiphenyl. 4,4'-diisocyanate-3,3'-dimethylbiphenyl, acid anhydride, and a second catalyst are mixed and subjected to a third polymerization reaction to obtain isocyanate-terminated PI molecular chains; the acid anhydride is 4,4'-(hexafluoroisopropene) phthalic anhydride. The amino-terminated PUU molecular chains and isocyanate-terminated PI molecular chains are mixed and subjected to a fourth polymerization reaction to obtain a shape memory PI-PUU block copolymer. Graphene oxide, 3-(aminomethyl)-4,6-dimethylpyridine-2(1H)-one, a first organic solvent and a third catalyst were mixed and grafted to obtain graphene oxide covalently modified with 3-(aminomethyl)-4,6-dimethylpyridine-2(1H)-one. The shape memory PI-PUU block copolymer, 3-(aminomethyl)-4,6-dimethylpyridine-2(1H)-one covalently modified graphene oxide, and a second organic solvent were mixed and cured to obtain a hydrogen bond-enhanced graphene composite shape memory polymer.
2. The preparation method according to claim 1, characterized in that, The diisocyanate includes one or more of isophorone diisocyanate, 1,6-hexanediisocyanate, terephthalic diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate and phenyldimethyl diisocyanate. The diol includes one or more of polycarbonate diol and polytetramethylene ether diol; The first catalyst comprises dibutyltin dilaurate or stannous octoate; The molar ratio of the diisocyanate to the diol is 2:1; the mass of the first catalyst is 0.01 to 0.03 wt% of the total mass of the diisocyanate and the diol. The temperature of the first polymerization reaction is 70–100°C; the time of the first polymerization reaction is 2–4 hours.
3. The preparation method according to claim 1, characterized in that, The diacylhydrazine monomer includes one or more of adipic diacylhydrazine, oxalic diacylhydrazine, malonic diacylhydrazine, succinic diacylhydrazine, azelaic diacylhydrazine, and dodecanedicarboxylic diacylhydrazine; The molar ratio of the diisocyanate to the difunctional aminobiphenyl is 10:0.1-3; the molar ratio of the diisocyanate to the diacylhydrazine monomer is 10:2.6-5.
6. The temperature of the second polymerization reaction is 70–100°C; the time of the second polymerization reaction is 6–12 hours.
4. The preparation method according to claim 1, characterized in that, The second catalyst comprises N,N-dimethylcyclohexylamine and N-methylaniline; the mass ratio of N,N-dimethylcyclohexylamine to N-methylaniline is 2:1 to 3; The molar ratio of 4,4'-diisocyanate-3,3'-dimethylbiphenyl to acid anhydride is 1 to 2:1; the mass of the second catalyst is 0.01 to 0.03 wt% of the total mass of 4,4'-diisocyanate-3,3'-dimethylbiphenyl and acid anhydride. The temperature of the third polymerization reaction is 130–160°C; the time of the third polymerization reaction is 10–24 hours.
5. The preparation method according to claim 1, characterized in that, The temperature of the fourth polymerization reaction is 60–100°C; the time of the fourth polymerization reaction is 24–60 hours.
6. The preparation method according to claim 1, characterized in that, The first organic solvent includes N,N-dimethylformamide or N,N-dimethylacetamide; The third catalyst comprises 4-dimethylaminopyridine and N,N'-dicyclohexylcarbodiimide; the mass ratio of 4-dimethylaminopyridine to N,N'-dicyclohexylcarbodiimide is 2:1 to 3. The mass ratio of the graphene oxide to 3-(aminomethyl)-4,6-dimethylpyridin-2(1H)-one is 0.06:0.04 to 0.06; The mass ratio of graphene oxide to the third catalyst is 100:0.01 to 0.
03.
7. The preparation method according to claim 1 or 6, characterized in that, The grafting reaction temperature is 0–25°C; the grafting reaction time is 24–48 hours.
8. The preparation method according to claim 1, characterized in that, The second organic solvent includes N,N-dimethylformamide or N,N-dimethylacetamide; The mass ratio of the shape memory PI-PUU block copolymer and the 3-(aminomethyl)-4,6-dimethylpyridine-2(1H)-one covalently modified graphene oxide is 100:0.1-2.
9. The hydrogen bond-enhanced graphene composite shape memory polymer prepared by the preparation method according to any one of claims 1 to 8.
10. The application of the hydrogen bond-enhanced graphene composite shape memory polymer of claim 9 in the preparation of functional coatings, wearable electronic devices, soft robots, electronic skin, or artificial muscles.
Citation Information
Patent Citations
Hydrophobic-heat-insulating-flame-retardant integrated aerogel composite material and preparation method thereof
CN121136438A