A heat treatment quenching and deep cryogenic tempering method for GCr15 ultra-precise miniature bearing steel ball

By employing a deep cryogenic tempering treatment method for GCr15 ultra-precision miniature bearing steel balls, the problems of high residual austenite content and large carbide particle size in domestically produced bearing steel balls have been solved, resulting in a significant improvement in hardness and dimensional stability, thus meeting the requirements of high-end equipment.

CN118222800BActive Publication Date: 2026-11-20INTELLIGENT MFG INST OF HFUT +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410291711.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-14
Publication Date
2026-11-20
Estimated Expiration
2044-03-14

AI Technical Summary

Technical Problem

The high residual austenite content and large carbide particle size of domestically produced precision miniature bearing steel balls result in poor dimensional stability, high noise, low fatigue life, and poor wear resistance, failing to meet the precision and service life requirements of high-end miniature intelligent equipment.

Method used

The heat treatment method of GCr15 ultra-precision miniature bearing steel balls, including quenching, precooling, cryogenic treatment and low temperature tempering, is adopted. By adding the cryogenic treatment process to the traditional process, the content of residual austenite is reduced and the particle size of carbides is improved.

Benefits of technology

The residual austenite content is significantly reduced to 4-5 vol%, the hardness is increased to 66-68 HRC, and the average particle size of carbides is reduced by 0.05 μm, which improves the dimensional stability and wear resistance of miniature bearing steel balls.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118222800B_ABST
    Figure CN118222800B_ABST
Patent Text Reader

Abstract

The application relates to the technical field of precision bearing machining, and discloses a heat treatment quenching deep cryogenic tempering treatment method for GCr15 super-precision micro bearing steel balls, which comprises the following steps: quenching; pre-cooling treatment; deep cryogenic treatment; low-temperature tempering; detection, analysis and characterization. According to the service state of high dimensional precision and stability and the use characteristics of high wear resistance of the micro bearing steel ball, the GCr15 super-precision micro bearing steel ball is subjected to quenching, liquid nitrogen deep cryogenic treatment and low-temperature tempering treatment, so that the residual austenite content of the GCr15 super-precision micro bearing steel ball after heat treatment can be greatly reduced, the hardness, wear resistance and dimensional stability can be improved, and the average particle size of carbide can be improved. After the above process treatment, the residual austenite content is reduced to 4-5 vol%, the hardness reaches 66-68 HRC, the average particle size of carbide is reduced by 0.05 um, and the dimensional stability of the micro bearing steel ball is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of precision bearing processing technology, and in particular to a heat treatment method for quenching and deep cryogenic tempering of GCr15 ultra-precision miniature bearing steel balls. Background Technology

[0002] In recent years, high-end micro-intelligent equipment has developed rapidly, and its rotating systems use a large number of precision micro-bearings. The most critical component that determines its precision and service life is the ultra-precision micro-bearing steel ball (a steel ball with a diameter of less than 2mm).

[0003] High-carbon chromium bearing steel GCr15, after conventional heat treatment, typically contains about 10 vol% retained austenite. Retained austenite is a relatively soft metastable phase, which can transform into martensite under certain service conditions, such as high stress and high friction. This changes the dimensional accuracy of the parts, potentially causing the bearing to malfunction.

[0004] For a long time, the microstructure of domestically produced precision miniature bearing steel balls has been inferior to that of foreign products, with a higher content of retained austenite and larger carbide particle size. This results in poor dimensional stability, high noise and interference, low fatigue life, and poor dynamic performance and wear resistance of domestically produced steel balls. There is an urgent need to develop a new process that can reduce retained austenite and carbide particle size.

[0005] Currently, a common method to reduce the residual austenite content and improve carbide particle size in bearing steel is to add cryogenic treatment to the traditional heat treatment process. During cryogenic treatment, the low temperature causes the residual austenite in the microstructure to decompose into martensite, while also causing ultrafine carbides to precipitate from the coarse martensite, resulting in dispersion strengthening and improved dimensional stability and wear resistance.

[0006] This invention improves the dimensional stability and wear resistance of ultra-precision miniature bearing steel balls by adding a deep cryogenic treatment process to the traditional quenching and tempering heat treatment process of GCr15 ultra-precision miniature bearing steel balls. This reduces the residual austenite content and improves the carbide particle size. Summary of the Invention

[0007] To address the technical problems mentioned in the background section, this invention provides a heat treatment method for quenching and deep cryogenic tempering of GCr15 ultra-precision miniature bearing steel balls.

[0008] This invention is achieved using the following technical solution: a method for heat treatment, quenching, and deep cryogenic tempering of GCr15 ultra-precision miniature bearing steel balls, comprising the following steps:

[0009] Quenching;

[0010] Pre-cooling treatment;

[0011] Cryogenic treatment;

[0012] Low-temperature tempering;

[0013] Detection, analysis, and characterization.

[0014] As a further improvement to the above solution, the quenching includes the following steps:

[0015] GCr15 ultra-precision miniature bearing steel balls with a diameter of 1.5mm are sealed and stored in glass tubes with a thickness of 2mm to prevent oxidation and decarburization during the heating process.

[0016] Turn on the box-type resistance furnace and heat to 800-860℃;

[0017] Place the glass tube containing the miniature bearing steel balls in a box-type resistance furnace, close the furnace door, and maintain the temperature for 20 minutes.

[0018] Pour the special quenching oil for bearing steel balls into the quenching bucket, take out the heated glass tube, quickly use crucible tongs to break the glass tube in the air, pour the heated miniature bearing steel balls into the quenching oil, and perform rapid quenching for 10 minutes.

[0019] After quenching, the GCr15 ultra-precision miniature bearing steel balls are taken out of the quenching oil and washed with detergent and water.

[0020] As a further improvement to the above scheme, the quenching is carried out in a KSL-1500X-S box-type resistance furnace, and the quenching medium is bearing steel ball quenching oil.

[0021] As a further improvement to the above solution, the pre-cooling process includes the following steps:

[0022] Open the freezer and set the temperature to -80℃.

[0023] Place the GCr15 ultra-precision miniature bearing steel ball in a crucible, then place the crucible containing the steel ball in a freezing oven and keep it at that temperature for 10 minutes to complete the pre-cooling.

[0024] As a further improvement to the above solution, the cryogenic treatment is carried out in a rotating liquid nitrogen cryogenic tank and includes the following steps:

[0025] 10L of liquid nitrogen was placed in a rotating liquid nitrogen cryogenic tank and kept at a constant temperature of -196℃;

[0026] After pre-cooling, GCr15 ultra-precision miniature bearing steel balls are loaded into a lifting bucket with holes at the bottom. The lifting bucket is then slowly and vertically lowered into a rotating liquid nitrogen cryogenic tank to submerge the GCr15 ultra-precision miniature bearing steel balls in liquid nitrogen. The lid of the rotating liquid nitrogen tank is then closed, and the temperature is kept constant at -196℃.

[0027] Turn on the motor switch of the rotating liquid nitrogen cryogenic tank to make the lifting bucket rotate at a speed of 10 r / min;

[0028] The liquid nitrogen cryogenic treatment time is 2 hours;

[0029] After rewarming and cryogenic treatment, the GCr15 ultra-precision miniature bearing steel balls are taken out and placed in the air for 10 minutes to allow them to return to 25°C.

[0030] As a further improvement to the above solution, the low-temperature tempering is carried out in a drying oven and includes the following steps:

[0031] Turn on the drying oven and heat it up, maintaining the temperature at 150℃;

[0032] The cryogenically cooled GCr15 ultra-precision miniature bearing steel balls were placed in a drying oven and kept at that temperature for 2 hours.

[0033] After the tempering time is reached, turn off the power to the drying oven and allow the steel balls to cool to 25°C with the furnace.

[0034] After tempering, remove the GCr15 ultra-precision miniature bearing steel balls.

[0035] As a further improvement to the above scheme, the detection, analysis, and characterization include the following steps:

[0036] After quenching steel balls at different temperatures by wire cutting, radial cutting, mounting, and polishing, the balls were etched with 4% nitric acid alcohol. The microstructure was observed under scanning electron microscope (SEM) and confocal microscope (CLSM), and the size of carbide particles was counted using Image Pro Plus software.

[0037] The residual austenite content was calculated using X-ray diffraction (XRD) according to the five-line, six-pair method specified in YB / T 5338-2019, "Quantitative Determination of Austenite in Steel by X-ray Diffraction". To avoid the influence of stress generated by grinding and polishing on the XRD parameter results, the sample preparation steps were as follows: the sample was first ground and polished, then etched with 4% nitric acid alcohol for 15 seconds, and then lightly polished with 0.02 μm silica suspension (OP-S) until the surface was bright. This process was repeated twice to remove stress.

[0038] Hardness was tested using an automatic Rockwell hardness tester with a loading force of 200g.

[0039] As a further improvement to the above scheme, the rotating liquid nitrogen cryogenic tank is a vertical cylindrical shape. The outermost part of the rotating liquid nitrogen cryogenic tank is an outer insulation shell (1), and the inside is a liquid nitrogen tank (3) with a feeding channel. Between the outer insulation shell (1) and the liquid nitrogen tank (3) is an inner insulation material (2). Liquid nitrogen (4) is contained in the liquid nitrogen tank (3). The liquid nitrogen tank (3) is placed with a lifting bucket (6) with a rotating stirring function through the feeding channel. It is sealed and cryogenically treated through the cryogenic tank cover (5).

[0040] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0041] The advantages of this invention compared to traditional miniature bearing steel ball technology are obvious. Based on the high dimensional accuracy and stability required for service and the high wear resistance of miniature bearing steel balls, this invention employs quenching, rapid cooling, liquid nitrogen cryogenic treatment, and low-temperature tempering on GCr15 ultra-precision miniature bearing steel balls. This significantly reduces the residual austenite content after heat treatment, improves hardness and wear resistance, and reduces the average carbide particle size. After the above process, the residual austenite content is reduced to 4-5 vol%, the hardness reaches 66-68 HRC, and the average carbide particle size is reduced by 0.05 μm, greatly improving the dimensional stability of the miniature bearing steel balls. The method proposed in this invention adds a cryogenic treatment process to the traditional bearing steel ball heat treatment method. This method is advanced, verified to have good treatment effect and strong process stability, and is an ideal and reliable method for heat treatment, quenching, cryogenic tempering, and treatment of miniature bearing steel balls. This method can also be extended to treat other bearing steels accordingly. Attached Figure Description

[0042] Figure 1 Diagram showing the cryogenic treatment state of GCr15 miniature bearing steel balls;

[0043] Figure 2 Figure 1. Residual austenite content of GCr15 miniature bearing steel balls before and after cryogenic treatment;

[0044] Figure 3 Comparison of average carbide particle size of GCr15 miniature bearing steel balls before and after cryogenic treatment;

[0045] Figure 4 Comparison of hardness of GCr15 miniature bearing steel balls before and after cryogenic treatment.

[0046] Explanation of key symbols:

[0047] 1. Outer insulation shell, 2. Inner insulation material, 3. Liquid nitrogen tank, 4. Liquid nitrogen, 5. Liquid nitrogen, 6. Lifting bucket. Detailed Implementation

[0048] The present invention will now be further described in conjunction with the accompanying drawings and specific embodiments. It should be noted that, without conflict, the various embodiments or technical features described below can be arbitrarily combined to form new embodiments.

[0049] Example 1:

[0050] In this embodiment, Figure 1 The image shows the state of the GCr15 ultra-precision miniature bearing steel ball during cryogenic treatment, with the positions of each part as shown in the figure.

[0051] The amount of chemical substances used in the cryogenic treatment of low-temperature nickel steel is determined according to a pre-set range, with units of measurement in millimeters and milliliters.

[0052] The cryogenic treatment of GCr15 ultra-precision miniature bearing steel balls is carried out in a rotating liquid nitrogen cryogenic tank:

[0053] The rotating liquid nitrogen cryogenic tank is a vertical cylindrical shape. The outermost part of the rotating liquid nitrogen cryogenic tank is an outer insulation shell (1), and the innermost part is a liquid nitrogen tank (3) with a feeding channel. Between the outer insulation shell (1) and the liquid nitrogen tank (3) is an inner insulation material (2). Liquid nitrogen (4) is contained in the liquid nitrogen tank (3). The liquid nitrogen tank (3) is placed with a lifting bucket (6) with a rotating stirring function through the feeding channel. The tank is sealed and cryogenic treatment is carried out through the cryogenic tank cover (5).

[0054] like Figure 2 The figure shows the residual austenite content of miniature bearing steel balls before and after cryogenic treatment. QT represents the content after quenching and tempering, and QCT represents the content after cryogenic treatment. It can be seen from the figure that the residual austenite content of miniature bearing steel balls is significantly reduced after cryogenic treatment.

[0055] like Figure 3 As shown in the figure, the average particle size of carbides in miniature bearing steel balls before and after cryogenic treatment is shown. QT represents the size after quenching and tempering, and QCT represents the size after cryogenic treatment. It is clear from the figure that the average particle size of carbides decreases after cryogenic treatment.

[0056] like Figure 4 The image shows a comparison of the hardness of miniature bearing steel balls before and after cryogenic treatment. QT represents the hardness after quenching and tempering, and QCT represents the hardness after cryogenic treatment. It can be seen that the hardness increases significantly after cryogenic treatment.

[0057] This embodiment refers to Figure 1-4 This document describes a heat treatment method for quenching and deep cryogenic tempering of GCr15 ultra-precision miniature bearing steel balls, comprising the following steps:

[0058] Quenching; the quenching is carried out in a KSL-1500X-S box-type resistance furnace, and the quenching medium is bearing steel ball quenching oil.

[0059] The quenching process includes the following steps:

[0060] GCr15 ultra-precision miniature bearing steel balls with a diameter of 1.5mm are sealed and stored in glass tubes with a thickness of 2mm to prevent oxidation and decarburization during the heating process.

[0061] Turn on the box-type resistance furnace and heat to 800-860℃;

[0062] Place the glass tube containing the miniature bearing steel balls in a box-type resistance furnace, close the furnace door, and maintain the temperature for 20 minutes.

[0063] Pour the special quenching oil for bearing steel balls into the quenching bucket, take out the heated glass tube, quickly use crucible tongs to break the glass tube in the air, pour the heated miniature bearing steel balls into the quenching oil, and perform rapid quenching for 10 minutes.

[0064] After quenching, the GCr15 ultra-precision miniature bearing steel balls are taken out of the quenching oil and washed with detergent and water.

[0065] Pre-cooling treatment;

[0066] The precooling process includes the following steps:

[0067] Open the freezer and set the temperature to -80℃.

[0068] Place the GCr15 ultra-precision miniature bearing steel ball in a crucible, then place the crucible containing the steel ball in a freezing oven and keep it at that temperature for 10 minutes to complete the pre-cooling.

[0069] Cryogenic treatment;

[0070] The cryogenic treatment is carried out in a rotating liquid nitrogen cryogenic tank and includes the following steps:

[0071] 10L of liquid nitrogen was placed in a rotating liquid nitrogen cryogenic tank and kept at a constant temperature of -196℃;

[0072] After pre-cooling, GCr15 ultra-precision miniature bearing steel balls are loaded into a lifting bucket with holes at the bottom. The lifting bucket is then slowly and vertically lowered into a rotating liquid nitrogen cryogenic tank to submerge the GCr15 ultra-precision miniature bearing steel balls in liquid nitrogen. The lid of the rotating liquid nitrogen tank is then closed, and the temperature is kept constant at -196℃.

[0073] Turn on the motor switch of the rotating liquid nitrogen cryogenic tank to make the lifting bucket rotate at a speed of 10 r / min;

[0074] The liquid nitrogen cryogenic treatment time is 2 hours;

[0075] In this scheme, the rotating liquid nitrogen cryogenic tank is a vertical cylindrical shape. The outermost part of the rotating liquid nitrogen cryogenic tank is an outer insulation shell (1), and the inside is a liquid nitrogen tank (3) with a feeding channel. Between the outer insulation shell (1) and the liquid nitrogen tank (3) is an inner insulation material (2). Liquid nitrogen (4) is contained in the liquid nitrogen tank (3). The liquid nitrogen tank (3) is placed with a lifting bucket (6) with a rotating stirring function through the feeding channel. It is sealed and cryogenically treated through the cryogenic tank cover (5).

[0076] After rewarming and cryogenic treatment, the GCr15 ultra-precision miniature bearing steel balls are taken out and placed in the air for 10 minutes to allow them to return to 25°C.

[0077] Low-temperature tempering;

[0078] The low-temperature tempering is carried out in a drying oven and includes the following steps:

[0079] Turn on the drying oven and heat it up, maintaining the temperature at 150℃;

[0080] The cryogenically cooled GCr15 ultra-precision miniature bearing steel balls were placed in a drying oven and kept at that temperature for 2 hours.

[0081] After the tempering time is reached, turn off the power to the drying oven and allow the steel balls to cool to 25°C with the furnace.

[0082] After tempering, remove the GCr15 ultra-precision miniature bearing steel balls.

[0083] Detection, analysis, and characterization.

[0084] The detection, analysis, and characterization include the following steps:

[0085] After quenching steel balls at different temperatures by wire cutting, radial cutting, mounting, and polishing, the balls were etched with 4% nitric acid alcohol. The microstructure was observed under scanning electron microscope (SEM) and confocal microscope (CLSM), and the size of carbide particles was counted using Image Pro Plus software.

[0086] The residual austenite content was calculated using X-ray diffraction (XRD) according to the five-line, six-pair method specified in YB / T 5338-2019, "Quantitative Determination of Austenite in Steel by X-ray Diffraction". To avoid the influence of stress generated by grinding and polishing on the XRD parameter results, the sample preparation steps were as follows: the sample was first ground and polished, then etched with 4% nitric acid alcohol for 15 seconds, and then lightly polished with 0.02 μm silica suspension (OP-S) until the surface was bright. This process was repeated twice to remove stress.

[0087] Hardness was tested using an automatic Rockwell hardness tester with a loading force of 200g.

[0088] The above embodiments are merely preferred embodiments of the present invention and should not be construed as limiting the scope of protection of the present invention. Any non-substantial changes and substitutions made by those skilled in the art based on the present invention shall fall within the scope of protection claimed by the present invention.

Claims

1. A method for heat treatment, quenching, and deep cryogenic tempering of GCr15 ultra-precision miniature bearing steel balls, characterized in that, Includes the following steps: Quenching; Pre-cooling treatment; Cryogenic treatment; Low-temperature tempering; Detection, analysis, and characterization; The precooling process includes the following steps: Open the freezer and set the temperature to -80℃. Place the GCr15 ultra-precision miniature bearing steel ball in a crucible, then place the crucible containing the steel ball in a freezing oven and keep it at that temperature for 10 minutes to complete the pre-cooling. The cryogenic treatment is carried out in a rotating liquid nitrogen cryogenic tank and includes the following steps: 10L of liquid nitrogen was placed in a rotating liquid nitrogen cryogenic tank and kept at a constant temperature of -196℃; After pre-cooling, GCr15 ultra-precision miniature bearing steel balls are loaded into a lifting bucket with holes at the bottom. The lifting bucket is then slowly and vertically lowered into a rotating liquid nitrogen cryogenic tank to submerge the GCr15 ultra-precision miniature bearing steel balls in liquid nitrogen. The lid of the rotating liquid nitrogen tank is then closed, and the temperature is kept constant at -196℃. Turn on the motor switch of the rotating liquid nitrogen cryogenic tank to make the lifting bucket rotate at a speed of 10 r / min; The liquid nitrogen cryogenic treatment time is 2 hours; After rewarming and cryogenic treatment, the GCr15 ultra-precision miniature bearing steel ball is taken out and placed in the air for 10 minutes to allow it to return to 25°C. The low-temperature tempering is carried out in a drying oven and includes the following steps: Turn on the drying oven and heat it up, maintaining the temperature at 150℃; The cryogenically cooled GCr15 ultra-precision miniature bearing steel balls were placed in a drying oven and kept at that temperature for 2 hours. After the tempering time is reached, turn off the power to the drying oven and allow the steel balls to cool to 25°C with the furnace. After tempering, remove the GCr15 ultra-precision miniature bearing steel balls.

2. The heat treatment, quenching, and deep cryogenic tempering method for GCr15 ultra-precision miniature bearing steel balls as described in claim 1, characterized in that, The quenching process includes the following steps: GCr15 ultra-precision miniature bearing steel balls with a diameter of 1.5mm are sealed and stored in glass tubes with a thickness of 2mm to prevent oxidation and decarburization during the heating process. Turn on the box-type resistance furnace and heat to 800-860℃; Place the glass tube containing the miniature bearing steel balls in a box-type resistance furnace, close the furnace door, and maintain the temperature for 20 minutes. Pour the special quenching oil for bearing steel balls into the quenching bucket, take out the heated glass tube, quickly use crucible tongs to break the glass tube in the air, pour the heated miniature bearing steel balls into the quenching oil, and perform rapid quenching for 10 minutes. After quenching, the GCr15 ultra-precision miniature bearing steel balls are taken out of the quenching oil and washed with detergent and water.

3. The heat treatment, quenching, and deep cryogenic tempering method for GCr15 ultra-precision miniature bearing steel balls as described in claim 1, characterized in that... The quenching was carried out in a KSL-1500X-S box-type resistance furnace, and the quenching medium was bearing steel ball quenching oil.

4. The heat treatment, quenching, and deep cryogenic tempering method for GCr15 ultra-precision miniature bearing steel balls as described in claim 1, characterized in that... The detection, analysis, and characterization include the following steps: After quenching steel balls at different temperatures by wire cutting, radial cutting, mounting, and polishing, the balls were etched with 4% nitric acid alcohol. The microstructure was observed under scanning electron microscopy (SEM) and confocal microscopy (CLSM), and the size of carbide particles was counted using ImagePro Plus software. The residual austenite content was calculated using X-ray diffraction (XRD) according to the five-line, six-pair method specified in YB / T 5338-2019 Quantitative Determination of Austenite in Steel by X-ray Diffraction. To avoid the influence of stress generated by grinding and polishing on the XRD parameter results, the sample preparation steps were as follows: first, the sample was ground and polished, then etched with 4% nitric acid alcohol for 15 seconds, and then lightly polished with 0.02 μm silica suspension (OP-S) until the surface was bright. This process was repeated twice to remove stress. Hardness was tested using an automatic Rockwell hardness tester with a loading force of 200g.

5. The heat treatment, quenching, and deep cryogenic tempering method for GCr15 ultra-precision miniature bearing steel balls as described in claim 1, characterized in that... The rotating liquid nitrogen cryogenic tank is a vertical cylindrical shape. The outermost part of the rotating liquid nitrogen cryogenic tank is an outer insulation shell (1), and the inside is a liquid nitrogen tank (3) with a feeding channel. Between the outer insulation shell (1) and the liquid nitrogen tank (3) is an inner insulation material (2). Liquid nitrogen (4) is contained in the liquid nitrogen tank (3). The liquid nitrogen tank (3) is placed with a lifting bucket (6) with a rotating stirring function through the feeding channel. The tank is sealed and cryogenic treatment is carried out through the cryogenic tank cover (5).

Citation Information

Patent Citations

  • Quenching / subzero treatment method for heat treatment of low-temperature nickel steel

    CN103343202A

  • Heat treatment residual austenite control process

    CN115584377A