A multi-element thermoelectric material and a method for producing the same
Patent Information
- Application Number
- CN202310468675.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-04-27
AI Technical Summary
此外,以前研究均通过高温熔融法制备EuMg2Sb2基材料,该方法耗能高、耗时长,不利于EuMg2Sb2材料的进一步发展
Smart Images

Figure CN118222865B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of thermoelectric energy conversion materials, specifically relating to a multi-element thermoelectric material and its preparation method. Background Technology
[0002] Thermoelectric conversion technology enables the direct conversion between heat energy and electrical energy, and has the potential applications in waste heat recovery, electronic component cooling, and other fields. Thermoelectric devices are typically composed of a series of n-type and p-type semiconductor materials. The thermoelectric conversion capability of these semiconductors is usually measured by the dimensionless thermoelectric figure of merit zT, where zT = S. 2 σT / κ, where S is the Seebeck coefficient, σ is the conductivity, and S 2 σ is the power factor, T is the absolute temperature, and κ is the thermal conductivity. Since the 1990s, many thermoelectric researchers have been keen to develop novel thermoelectric materials with "phonon glass-electron crystal" (PGEC) characteristics, among which the Zintl phase system has been extensively and deeply studied. One of the main Zintl phase systems, the "1-2-2" type Zintl phase, has seen continuous breakthroughs reported in recent years. However, these results are mostly concentrated on n-type Mg3Sb2-based thermoelectric materials. Although p-type EuMg2Sb2-based materials have the potential to be assembled with n-type Mg3Sb2-based materials into thermoelectric devices, the poor intrinsic electrical transport properties of EuMg2Sb2 result in a relatively low zT.
[0003] In recent years, researchers have optimized the carrier concentration and thermal conductivity of EuMg2Sb2 material through Na doping, ultimately obtaining a peak zT of 0.8, which is comparable to the zT value of the best p-type Mg3Sb2-based material, showing good prospects for EuMg2Sb2-based materials in the thermoelectric field. However, EuMg2Sb2 material has a large band gap, making heterovalent doping less effective. In contrast, the crystal structure of AB2Sb2 (A = Eu, Yb, B = Zn) compound is consistent with that of EuMg2Sb2, and it is highly feasible to improve the thermoelectric transport performance of EuMg2Sb2 compound by solid solution of AB2Sb2: (1) In terms of electrical transport performance, solid solution of AB2Sb2 is expected to weaken the polarity of the anionic framework, which is conducive to carrier transport; (2) In terms of thermal transport performance, the additional point defects introduced by solid solution of AB2Sb2 can enhance the scattered phonons, which is expected to reduce the lattice thermal conductivity. Furthermore, previous studies have all prepared EuMg2Sb2-based materials using a high-temperature melting method, which is energy-intensive and time-consuming, hindering the further development of EuMg2Sb2 materials. To promote the rapid development of EuMg2Sb2-based thermoelectric materials, it is necessary to introduce more energy-efficient and faster synthesis methods. Summary of the Invention
[0004] To address the aforementioned problems in the existing technology, the present invention aims to provide a method for preparing Eu-Yb-Mg-Zn-Sb multi-element thermoelectric materials that features low energy consumption, short preparation time, and excellent thermoelectric performance.
[0005] To solve the above-mentioned technical problems, the present invention adopts the following technical solution: a method for preparing a multi-element thermoelectric material, specifically with the chemical formula Eu. 1-y Yb y Mg 2.2(1-x) Zn 2x Sb2 includes the following steps:
[0006] S1: In a glove box filled with argon gas, according to the chemical formula Eu 1-y Yb y Mg 2.2(1-x) Zn 2x To prepare Sb2, weigh out Eu flakes, Yb powder, Mg powder, Zn granules, and Sb powder and add them to a ball mill jar, where x = 0–0.5 and y = 0–0.5. Then seal the ball mill jar. A sealing film can be used at the jar opening to ensure good sealing. The ball-to-material ratio in the ball mill jar is 5:1 to 10:1.
[0007] S2: Remove the grinding jar from the glove box and place it into the high-energy ball mill in an air atmosphere. Grind for 50–70 minutes, the grinding time of which can be 50, 60, or 70 minutes. The rotation speed of the ball mill is 1500 r / min.
[0008] S3: Remove the ball mill jar from the high-energy ball mill, place it in an argon-filled glove box, open the ball mill jar, crush the sediment at the bottom of the jar, remix all the powder inside the jar evenly, and reseal the ball mill jar.
[0009] S4: Repeat the processes of S2 and S3. High-energy ball milling utilizes external mechanical energy to promote the reaction. At the same time, the presence of the S3 process ensures the quality of ball milling. The chemical reaction proceeds rapidly. Therefore, the total ball milling time is 180 min to 280 min to complete the chemical reaction. The total ball milling time can be 180 min, 200 min, 210 min, 240 min, 250 min, or 280 min.
[0010] S5: After the ball milling process is complete, open the milling jar in an argon-filled glove box, remove the sample, place it in an agate mortar, and grind it to obtain sample powder. The grinding time is 4–10 minutes, preferably 5 minutes.
[0011] S6: Place the powder in a graphite mold, with thin carbon paper at both ends. After loading, remove the mold from the argon atmosphere and place it on a hot press for sintering to obtain a bulk Eu-Yb-Mg-Zn-Sb multi-element thermoelectric material. The sintering temperature is 620–650℃, the sintering pressure is 40–60 MPa, and the holding time is 20–40 min. The sintering temperature can be 620℃, 630℃, 640℃, or 650℃; the sintering pressure can be 40 MPa, 50 MPa, or 60 MPa; and the holding time can be 20 min, 30 min, or 40 min.
[0012] Preferably, the grinding jar contains two sizes of grinding balls, with a ratio of large-diameter grinding balls to small-diameter grinding balls of 2:1 to 1:1. After the raw material is weighed, two 1 / 2-inch diameter stainless steel balls and two to four 1 / 4-inch diameter stainless steel balls are placed inside. Two, three, or four 1 / 4-inch balls can be used.
[0013] Preferably, the ball-to-material ratio in S1 is 5:1.
[0014] A multi-element thermoelectric material, chemically represented as Eu 1-y Yb y Mg 2.2(1-x) Zn 2x Sb2 was prepared using the method described above.
[0015] Specifically, x = 0, 0.1, 0.2, 0.3, 0.4 or 0.5, and y = 0, 0.1, 0.3 or 0.5.
[0016] Compared with the prior art, the present invention has at least the following advantages:
[0017] 1. This invention uses a high-energy ball milling method to prepare p-type Eu-Yb-Mg-Zn-Sb multi-element thermoelectric materials. Compared with the traditional high-temperature melting method, it takes less time, consumes less energy, and the entire preparation process is highly efficient, enabling rapid and large-scale sample preparation.
[0018] 2. This invention can achieve a large proportion and uniform solid solution. By changing the proportion of solid solution elements, the thermoelectric properties of EuMg2Sb2-based materials are significantly optimized, and the electrical transport properties are highly adjustable. For example, by adjusting the composition, the electrical conductivity of EuMg2Sb2 can be increased by several thousand times, which is beneficial to the practical application of EuMg2Sb2-based materials.
[0019] 3. This invention creatively performs solid solution alloying at both the Eu and Mg sites in EuMg2Sb2, which greatly improves the electrical conductivity of the material and significantly optimizes the power factor. At the same time, the solid solution introduces a large number of point defects, which effectively reduces the lattice thermal conductivity. Ultimately, the zT of EuMg2Sb2 material is improved across the entire temperature range, with the peak zT reaching 1.01 at 823K, which is the highest zT value for EuMg2Sb2-based thermoelectric materials to date. Attached Figure Description
[0020] Figure 1 EuMg 2.2(1-x) Zn 2x Sb2(x=0,0.5) and Eu 1-y Yb y Mg 1.1 XRD patterns of ZnSb2 (y = 0.1, 0.3, 0.5) blocks.
[0021] Figure 2 EuMg 1.1 SEM images and EDX elemental distributions of ZnSb2 samples: (a) SEM image of sample cross-section, (b) SEM image of polished sample and (cf) corresponding EDX distributions of Eu, Mg, Zn and Sb.
[0022] Figure 3 EuMg 1.1 TGA results of ZnSb2 samples.
[0023] Figure 4 Eu in this invention 0.5 Yb 0.5 Mg 1.1 Comparison of the maximum zT values of ZnSb2 samples with some p-type AMG2Sb2-based materials reported in the literature.
[0024] Figure 5 This is a process flow diagram of the method of the present invention. Detailed Implementation
[0025] The present invention will now be described in further detail.
[0026] The electronegativity difference between Zn and Sb is smaller than that between Mg and Sb. Furthermore, the high carrier concentration in AZn₂Sb₂ (A = Eu, Yb) materials allows for Zn solid solution at Mg sites to weaken the electronegativity of [Mg₂Sb₂]. 2-The polarity of the anionic framework and the increase in carrier concentration are expected to effectively improve the electrical conductivity of EuMg2Sb2 materials. Studies have shown that the electronegativity difference between A-Sb affects the vacancy formation energy, and the electronegativity difference between Yb-Sb is smaller than that between Eu-Sb. Therefore, solid-solid ...
[0027] (1) This invention uses high-energy ball milling to prepare samples. Compared with the traditional melting method, ball milling requires less time and consumes less energy. Specifically, the traditional melting method requires heating the sample to 1150°C and holding it at that temperature for 2 hours, followed by quenching, and finally annealing at 900°C for 2 days, which is energy-intensive and time-consuming. In contrast, the high-energy ball milling method in this invention is carried out at room temperature, requiring 180-280 minutes. The reason for the improved preparation efficiency is that the high-energy ball milling method utilizes external mechanical energy to cause repeated collisions between the grinding balls and the powder. During this process, the powder is subjected to impact and shearing, which reduces the diffusion activation energy of the system, thereby achieving atomic diffusion, promoting the reaction, and achieving alloying in the solid state. Therefore, the high-energy ball milling method requires less preparation time than the high-temperature melting method. In addition, the strategy of opening the tank midway for uniform mixing in this invention further ensures the uniformity of elements, which is beneficial to improving the ball milling efficiency and further reducing the required ball milling time.
[0028] (2) In this invention, after each 50-70 minute ball milling process, the stainless steel ball mill jar is opened in the glove box to knock off, crush, and grind the deposits at the bottom of the jar. The powder is then remixed evenly before continuing ball milling. This process ensures the quality of ball milling, makes element solid solution time-saving and efficient, and ensures the phase purity and homogeneity of the synthesized sample while reducing ball milling time. Simultaneously, combined with a suitable sintering process, bulk samples are prepared, resulting in dense bulk samples with uniform distribution of all elements. Comparative experiments show that without the step of crushing the deposits midway, the chemical reaction cannot proceed completely, and the XRD pattern shows a significant Sb diffraction peak.
[0029] (3) Benefiting from the consistent crystal structure and rich and diverse composition of the 1-2-2 type Zintl phase, the types and amounts of solid solution elements are highly adjustable, which allows for a significant optimization of the thermoelectric properties of the material. This invention significantly optimizes the thermoelectric transport properties of EuMg2Sb2 material, with a peak zT reaching 1.01, making it one of the best-performing p-type AMg2Sb2-based materials in terms of thermoelectric performance.
[0030] During high-energy ball milling, powder particles are repeatedly welded and broken by impact, refining large particles into smaller ones. This increases the surface activity of the particles, facilitating solid-state reactions. Optimization theory requires the support of practical preparation methods. The method of this invention improves the efficiency of diffusion reactions during preparation, successfully achieving alloying. Optimization of material composition significantly enhances electrical transport properties. Furthermore, lattice defects generated during ball milling hinder phonon transport, thus reducing the sample's lattice thermal conductivity. Therefore, the multi-component thermoelectric material sample prepared by this invention exhibits excellent thermoelectric transport properties.
[0031] 1. Samples that only undergo Zn solid solution treatment at the Mg sites, i.e., samples with the chemical formula EuMg 2.2(1-x) Zn 2x Preparation of Sb2 materials:
[0032] The following will elaborate on EuMg 2.2(1-x) Zn 2x Preparation process of Sb2 (x=0,0.1,0.2,0.3,0.4,0.5) materials.
[0033] Example 1: EuMg 2.2 Sb2 material preparation process
[0034] S1: According to the stoichiometric ratio in the chemical formula, weigh 1.6940g of Eu sheet, 0.5955g of Mg powder and 2.7124g of Sb powder in a glove box filled with argon gas, add them to the ball mill jar, the ball-to-material ratio is 5:1, then seal the ball mill jar, and use a sealing film at the mouth of the jar to ensure good sealing.
[0035] S2: Remove the grinding jar from the glove box and place it into the high-energy ball mill in an air atmosphere. Set the grinding time to 60 minutes and the rotation speed to 1500 r / min.
[0036] S3: After the stage of ball milling is completed, remove the ball mill jar from the high-energy ball mill, put it into a glove box filled with argon, open the ball mill jar, crush the sediment at the bottom of the jar, remix all the powder evenly, and reseal the ball mill jar.
[0037] S4: Repeat the process of S2 and S3, with a 30-minute interval between each ball milling, for a total of 180 minutes of ball milling.
[0038] S5: After the ball milling process is completed, open the ball mill jar in an argon-filled glove box, take out the sample, place it in an agate mortar, and grind for 5 minutes to obtain a powder sample.
[0039] S6: Place the powder in a graphite mold, with thin carbon paper at both ends. After the sample is loaded, remove the mold from the argon atmosphere and place it on a hot press. Keep it at 50 MPa and 650℃ for 20 minutes to obtain a block sample.
[0040] The preparation process of Examples 2 to 6 is the same as that of Example 1, except that the ratio of raw materials and the selection of process parameters are different, as shown in Table 1.
[0041] It should be noted that processes S2 to S4 are all designed to maximize the advantages of high-energy ball milling and ensure that the chemical reaction is completed. After multiple tests, the inventors found that the chemical reaction can be completed completely by following the ball milling process parameters provided by S2 to S4, and the differences between them have a very small impact on thermoelectric performance.
[0042] Table 1
[0043]
[0044] 2. A sample with the chemical formula Eu, formed by the co-solid solution of Yb and Zn. 1-y Yb y Mg 2.2(1-x) Zn 2x Sb2:
[0045] After Zn is dissolved at the Mg site, the conductivity is further improved by dissolving Yb at the Eu site. The details of Eu are explained below. 1- y Yb y Mg 2.2(1-x) Zn 2x Sb2 (x can be 0.1 to 0.5, y can be 0.1 to 0.5) sample preparation process.
[0046] Example 7: Eu 0.9 Yb 0.1 Mg 1.98 Zn 0.1 Sb2 sample preparation process
[0047] S1: According to the stoichiometric ratio in the chemical formula, weigh out 1.5120g of Eu flakes, 0.1912g of Yb powder, 0.5320g of Mg powder, 0.0723g of Zn granules, and 2.6925g of Sb powder in sequence in a glove box filled with argon gas, and add them to the ball mill jar. The ball-to-material ratio is 5:1. Then seal the ball mill jar and use a sealing film at the mouth of the jar to ensure good sealing.
[0048] S2: Remove the grinding jar from the glove box and place it into the high-energy ball mill in an air atmosphere. Set the grinding time to 50 minutes and the rotation speed to 1500 r / min.
[0049] S3: After the stage of ball milling is completed, remove the ball mill jar from the high-energy ball mill, put it into a glove box filled with argon, open the ball mill jar, crush the sediment at the bottom of the jar, remix all the powder evenly, and reseal the ball mill jar.
[0050] S4: Repeat the process of S2 and S3, with a 30-minute interval between each ball milling, for a total of 200 minutes of ball milling.
[0051] S5: After the ball milling process is completed, open the ball mill jar in an argon-filled glove box, take out the sample, place it in an agate mortar, and grind for 5 minutes to obtain a powder sample.
[0052] S6: Place the powder in a graphite mold, with thin carbon paper at both ends. After the sample is loaded, remove the mold from the argon atmosphere and place it on a hot press. Keep it at 50 MPa and 650℃ for 30 minutes to obtain a block sample.
[0053] The preparation process of Examples 8 to 21 is the same as that of Example 7, except that the ratio of raw materials and the selection of process parameters are different, as shown in Table 2.
[0054] Table 2
[0055]
[0056] Figure 1 EuMg 2.2(1-x) Zn 2x Sb2(x=0,0.5) and Eu 1-y Yb y Mg 1.1 XRD patterns of ZnSb2 (x = 0.1, 0.3, 0.5) bulk materials. The results show that the diffraction peaks of all samples correspond well with hexagonal EuMg2Sb2 (PDF 97-041-2653) or EuZn2Sb2 (PDF 97-038-0375), and there are no impurity peaks, indicating the successful synthesis of Eu-Yb-Mg-Zn-Sb multi-component thermoelectric materials.
[0057] Figure 2 (a) is EuMg 1.1 SEM image of the cross-section of a ZnSb2 sample. Figure 2 (b) is EuMg 1.1 SEM image of a polished ZnSb2 sample. Figure 2 (cf) shows the corresponding EDX surface distributions of Eu, Mg, Zn, and Sb. The above results indicate that the synthesized EuMg... 1.1 The ZnSb2 bulk sample has a dense structure and a uniform distribution of constituent elements.
[0058] Figure 3 EuMg1.1 The TGA results of the ZnSb2 material show that the sample has no significant weight change in the temperature range of 300 to 1000 K, proving its good thermal stability.
[0059] Figure 4 The Eu in this invention is shown 0.5 Yb 0.5 Mg 1.1 The ZnSb2 sample exhibits the highest zT values reported in the literature for some p-type AMg2Sb2-based materials. It is evident that Eu... 0.5 Yb 0.5 Mg 1.1 The highest zT value of ZnSb2 reaches 1.01, which is advantageous compared to the zT values of other AMG2Sb2-based materials.
[0060] The inventors conducted thermoelectric performance tests on the Eu-Yb-Mg-Zn-Sb multi-element thermoelectric materials obtained in some embodiments. The test results at 823K are shown in Table 3:
[0061] Table 3
[0062]
[0063] Actual preparation of EuMg 2.2 The Sb2 sample exhibited extremely poor conductivity, exceeding the testing range of commercial equipment; therefore, the power factor and zT value of the sample were not obtained. Table 3 shows that: [The text abruptly ends here, likely due to an incomplete sentence or missing information.] 2.2 Solid solution of EuZn2Sb2 in Sb2 can synergistically optimize p-type EuMg 2.2 The thermoelectric properties of Sb2 are improved by simultaneously increasing the power factor and reducing the lattice thermal conductivity, thereby increasing the zT value of the sample. In the EuZn2Sb2 sample, the solid solution of Yb at the Eu site further improves the power factor and reduces the lattice thermal conductivity, thus achieving synergistic optimization of thermoelectric properties. The highest zT value of the corresponding material is increased to 1.01, which ranks among the top zT values of p-type AMG2Sb2-based thermoelectric materials.
[0064] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A method for preparing a multi-element thermoelectric material, characterized in that: The chemical formula of the multi-element thermoelectric material is Eu. 1- y Yb y Mg 2.2(1-x) Zn 2x The preparation process of Sb2 includes the following steps: S1: In a glove box filled with argon gas, according to the chemical formula Eu 1-y Yb y Mg 2.2(1-x) Zn 2x The stoichiometric ratio of Sb2 was determined by weighing Eu flakes, Yb powder, Mg powder, Zn granules, and Sb powder and adding them to a ball mill jar. x = 0.1 ~ 0.5, y = 0.1 ~ 0.5, then seal the ball mill jar, the ball-to-material ratio in the ball mill jar is 5:1~10:1; S2: Remove the grinding jar from the glove box and place it into the high-energy ball mill in an air atmosphere. Grind for 50-70 minutes. S3: Remove the ball mill jar from the high-energy ball mill, place it in an argon-filled glove box, open the ball mill jar, crush the sediment at the bottom of the jar, remix all the powder inside the jar evenly, and reseal the ball mill jar. S4: Repeat the process of S2 and S3, with a total ball milling time of 180 min to 280 min; S5: After the ball milling process is completed, open the ball mill jar in an argon-filled glove box, take out the sample, place it in an agate mortar, and grind it to obtain sample powder; S6: Place the powder in a graphite mold, with thin carbon paper at both ends. After the sample is loaded, remove the mold from the argon atmosphere and place it on a hot press for sintering to obtain Eu-Yb-Mg-Zn-Sb multi-element thermoelectric material bulk material. The sintering temperature is 620~650 ℃, the sintering pressure is 40~60 MPa, and the holding time is 20~40 min.
2. The method for preparing the multi-element thermoelectric material as described in claim 1, characterized in that: The grinding jar contains two sizes of grinding balls, with the ratio of large-diameter grinding balls to small-diameter grinding balls being 2:1 to 1:
1.
3. A Eu-Yb-Mg-Zn-Sb multi-element thermoelectric material, characterized in that: Prepared using the preparation method described in claim 1 or 2.
Citation Information
Patent Citations
P type europium zincium and stibium based thermoelectric material, preparation thereof
CN101359713A