A heavy distillate hydrofining catalyst and a method for preparing the same

By using a network structure support and organic complexing agent to adjust the distribution of active metals in the hydrogenation catalyst of heavy distillate oil, the problem of poor deep desulfurization and denitrification effect of existing catalysts has been solved, and a more efficient hydrogenation reaction effect has been achieved.

CN118237035BActive Publication Date: 2026-11-24PETROCHINA CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211670696.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-23
Publication Date
2026-11-24
Estimated Expiration
2042-12-23

AI Technical Summary

Technical Problem

Existing heavy distillate oil hydrotreating catalysts have limited effectiveness in deep hydrodesulfurization and denitrification, and uneven metal concentration distribution leads to high molecular diffusion resistance.

Method used

The carrier has a mesh-like structure with through holes. The active components, nickel oxide and/or cobalt oxide, are distributed in a decreasing manner from the surface to the interior of the carrier, while molybdenum oxide and/or tungsten oxide are uniformly distributed. The impregnation rate and distribution of the active metals are adjusted by an organic complexing agent to form an eggshell-shaped structure.

Benefits of technology

It improves the deep hydrodesulfurization and denitrification activity of the catalyst, reduces steric hindrance, enhances hydrogen overflow effect, and achieves a more efficient hydrogenation reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004013779300000091
    Figure BDA0004013779300000091
  • Figure HDA0004013779310000011
    Figure HDA0004013779310000011
  • Figure HDA0004013779310000012
    Figure HDA0004013779310000012
Patent Text Reader

Abstract

This invention provides a catalyst for the hydrorefining of heavy distillate oil and its preparation method. The catalyst includes a support and an active component. The support has a network structure with interconnected pores. The active component includes nickel oxide and / or cobalt oxide, as well as molybdenum oxide and / or tungsten oxide. The nickel oxide and / or cobalt oxide are distributed in a decreasing manner from the surface to the interior of the support, while the molybdenum oxide and / or tungsten oxide are uniformly distributed on the support. This catalyst exhibits high activity for deep hydrodesulfurization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of heavy oil hydrogenation technology, specifically relating to a heavy distillate oil hydrogenation refining catalyst and its preparation method. Background Technology

[0002] Global standards for vehicle fuels are becoming increasingly stringent. The National VI diesel standard was implemented nationwide on January 1, 2019. Simultaneously, the increasing use of heavier feedstocks and the growing volume of sulfur-containing and high-sulfur crude oil processed by petrochemical companies have also posed challenges to upgrading diesel quality. Hydrogenation technology is the most effective method for producing clean diesel. Currently, the main methods for upgrading diesel quality to National VI standards for diesel hydrogenation units include reducing unit throughput, increasing the severity of the reaction, lowering the diesel's final boiling point, and using highly active diesel hydrogenation catalysts. Among these, highly active and selective catalysts are the most effective means to achieve a highly efficient hydrogenation process.

[0003] To adapt to the new requirements for diesel quality upgrading and the trend of crude oil becoming heavier, the development of highly active diesel hydrorefining catalysts remains a key research focus.

[0004] Application No. 201310533922.4 relates to a hydrotreating catalyst suitable for hydrodesulfurization of heavy distillate oil, its manufacturing method, and its application. This hydrotreating catalyst exhibits significantly improved activity in (deep) hydrodesulfurization of heavy distillate oil, but its deep hydrodenitrogenation effect is limited.

[0005] Application No. 200910086745.3 relates to a hydrogenation catalyst with a gradient distribution of active metal component concentration and its preparation method, which employs a saturation impregnation method to prepare the hydrogenation catalyst. This method involves preparing a relatively dilute solution of Group VIB and / or Group VIII metals or deionized water, and then gradually adding a more concentrated metal solution to saturate the support during the impregnation process; or preparing metal solutions of different concentrations and impregnating the support in ascending order of metal impregnation concentration. The catalyst prepared by this method exhibits an uneven metal concentration distribution, resulting in significant molecular diffusion resistance. Summary of the Invention

[0006] The purpose of this invention is to provide a catalyst for the hydrorefining of heavy distillate oil and its preparation method, which has high activity for deep hydrodesulfurization.

[0007] To achieve the above objectives, the present invention provides a heavy distillate oil hydrorefining catalyst, comprising a support and an active component, wherein the support has a network structure with through pores; the active component comprises nickel oxide and / or cobalt oxide and molybdenum oxide and / or tungsten oxide, wherein the nickel oxide and / or cobalt oxide are distributed in a decreasing manner from the surface to the interior of the support, and the molybdenum oxide and / or tungsten oxide are uniformly distributed on the support.

[0008] The heavy distillate oil hydrorefining catalyst of the present invention, based on 100% catalyst weight, contains 2-10% nickel oxide and / or cobalt oxide and 18-30% molybdenum oxide and / or tungsten oxide.

[0009] The heavy distillate oil hydrorefining catalyst of the present invention has a support comprising alumina and / or silica.

[0010] The heavy distillate oil hydrorefining catalyst of the present invention involves adding a cross-linked polymer during the preparation of the support, followed by calcination to ablate the cross-linked polymer, resulting in a through-pore structure with a network structure.

[0011] The heavy distillate oil hydrorefining catalyst of this invention uses a crosslinked polymer, which is one or more of polyvinyl alcohol-sodium polyacrylate, polyethylene glycol, and polypropylene glycol. The amount of the crosslinked polymer added is 4-8 wt% of the total amount of the carrier raw materials. In this invention, the crosslinked polymer has a network structure, which occupies positions during the extrusion molding process of the carrier preparation, and then forms a network structure at the occupied positions of the carrier after calcination and ablation.

[0012] The heavy distillate oil hydrorefining catalyst of the present invention also includes boron oxide added during the preparation of the support, wherein the amount of boron oxide added is 2-10 wt% of the total amount of the support raw materials.

[0013] To achieve the above objectives, the present invention also provides a method for preparing the heavy distillate oil hydrorefining catalyst, comprising the following steps:

[0014] S1, mix the carrier raw materials, add acid solution, and then extrude, shape, dry and calcine to obtain a carrier with a network of interconnected pores;

[0015] S2, mix the active component precursor, water, organic complexing agent and phosphorus-containing precursor to prepare an impregnation solution, impregnate the support, and then dry to obtain the finished catalyst.

[0016] In this invention, the addition of an organic complexing agent to the impregnation solution enables different diffusion rates of the metal within the catalyst pores. The organic complexing agent and the active metal form multi-metal complex clusters, weakening the strong metal-support interaction during impregnation and improving the dispersion of active metal atoms. During the impregnation process of this invention, a portion of the active component settles and adsorbs onto the pore wall surface, while another portion, or even all of the active component, remains in the solution within the pore volume. Utilizing the different diffusion rates of the organic complexing agent and the active metal solution on the support, the active component is redistributed as water evaporates and shifts in the solution.

[0017] The present invention does not impose any special limitation on the impregnation method, which is a conventional technical means in the field. Those skilled in the art can choose according to the actual situation. For example, the carrier can be impregnated by the equal amount impregnation method in the present invention.

[0018] The method for preparing the heavy distillate oil hydrorefining catalyst of the present invention comprises an organic complexing agent that is an organic acid and / or a polyol, wherein the organic acid is one or more of citric acid, oxalic acid and ascorbic acid, and the polyol is pentaerythritol and / or diethylene glycol.

[0019] In the preparation method of the heavy distillate oil hydrorefining catalyst of the present invention, the impregnation time in step S2 is 30-60 min, the drying temperature is 120-170℃, and the drying time is 4-8 h. In the present invention, the impregnation time and drying rate can further affect the distribution of active metals on the catalyst.

[0020] In the preparation method of the heavy distillate oil hydrorefining catalyst of the present invention, the acid solution in step S1 is a nitric acid solution or a phosphoric acid solution.

[0021] Beneficial effects of this invention:

[0022] Sulfur-containing compounds with steric hindrance do not readily enter the catalyst channels for reaction. Therefore, the distribution of cobalt / nickel near the outer surface of the catalyst channels is more conducive to benzene ring saturation before hydrodesulfurization. By adjusting the atomic ratio of Co(Ni) and Mo using the method of this invention, the relative content of Co(Ni) / Mo is higher than that inside the catalyst. This generates more Co(Ni)Sx species, such as Co9S8, which enhances surface hydrogen overflow. Consequently, the relative weight of hydrogen overflow and Co(Ni)-Mo-S in the catalyst performance varies with different catalyst cross-sections, achieving deep hydrodesulfurization and denitrification.

[0023] The interaction between the active metal component and the support affects the dispersibility and reducibility of the active metal component. Alumina supports exhibit strong interactions with transition metal oxides, making it easier for the active component to form less active type I metal sulfide structures, thus reducing catalyst activity. Silica has good stability and a large specific surface area, which can improve the dispersibility of the active component and enhance the catalyst's thermal stability; however, the interaction between silica and the active component is weak, hindering its dispersion. Using a mixture of alumina and silica as a composite support can regulate the interaction between the support and the active metal, forming more active type II metal sulfide structures and improving catalyst activity. Attached Figure Description

[0024] Figure 1 This is a concentration distribution diagram of the Co / Mo atomic ratio of the active metal component in the catalyst particles prepared in Example 2.

[0025] Figure 2 The concentration distribution of the active metal component Co / Mo atomic ratio on the catalyst particles prepared for Comparative Example 1 is shown in the figure. Detailed Implementation

[0026] The present invention will now be described in detail through embodiments. It should be noted that the following embodiments are only for further illustration of the present invention and should not be construed as limiting the scope of protection of the present invention. Those skilled in the art can make some non-essential improvements and adjustments to the present invention based on the above description.

[0027] Example 1

[0028] Step S1: Weigh 84g of alumina powder, 10g of boron oxide and 6g of polyvinyl alcohol-sodium polyacrylate cross-linked network hydrogel (molecular weight 20000), mix them in a kneader, add 100g of aqueous solution containing 2g of nitric acid dropwise during the kneading process, extrude into clover-shaped strips with a diameter of 1.3mm, dry at 120℃ for 4h, calcine at 500℃ for 4h to obtain catalyst support 1-A.

[0029] Step S2: Weigh 34.7g of molybdenum trioxide and 12.5g of basic cobalt carbonate, add deionized water, 5g of phosphoric acid, and 9g of citric acid, heat and stir until completely dissolved, cool to room temperature to obtain the impregnation solution. Impregnate 100g of the prepared carrier with the impregnation solution for 60min, let stand for 3h after impregnation, and dry at 150℃ for 4h to obtain the finished product 1-C.

[0030] Example 2

[0031] Step S1: Weigh 64g of alumina powder, add 20g of silica, 10g of boron oxide and 6g of polyvinyl alcohol-sodium polyacrylate cross-linked network hydrogel (molecular weight 20000), knead on a kneader, add 100g of aqueous solution containing 2g of nitric acid dropwise during kneading, extrude into clover-shaped strips with a diameter of 1.3mm, dry at 120℃ for 4h, calcine at 500℃ for 4h to obtain catalyst support 2-A.

[0032] Step S2: Weigh 34.7g of molybdenum trioxide and 12.5g of basic cobalt carbonate, add deionized water, 5g of phosphoric acid, and 9g of citric acid, heat and stir until completely dissolved, cool to room temperature to obtain the impregnation solution. Impregnate 100g of the prepared carrier with the impregnation solution for 60min, let stand for 3h after impregnation, and dry at 150℃ for 4h to obtain the finished product 2-C.

[0033] Example 3

[0034] Step S1: Weigh 64g of alumina powder, add 20g of silica, 10g of boron oxide and 6g of polypropylene glycol cross-linked network hydrogel (molecular weight 6000), knead on a kneader, add 100g of aqueous solution containing 2g of nitric acid dropwise during kneading, extrude into clover-shaped strips with a diameter of 1.3mm, dry at 120℃ for 4h, calcine at 500℃ for 4h to obtain catalyst support 3-A.

[0035] Step S2: Weigh 34.7g of molybdenum trioxide and 12.5g of basic cobalt carbonate, add deionized water, 5g of phosphoric acid, and 4.5g of citric acid, heat and stir until completely dissolved, cool to room temperature to obtain the impregnation solution. Impregnate 100g of the prepared carrier with the impregnation solution for 60min, let stand for 3h after impregnation, and dry at 150℃ for 4h to obtain the finished product 3-C.

[0036] Example 4

[0037] Step S1: Weigh 64g of alumina powder, add 20g of silica, 10g of boron oxide and 6g of polyvinyl alcohol-sodium polyacrylate cross-linked network hydrogel (molecular weight 20000), knead on a kneader, add 100g of aqueous solution containing 2g of nitric acid dropwise during kneading, extrude into clover-shaped strips with a diameter of 1.3mm, dry at 120℃ for 4h, calcine at 500℃ for 4h to obtain catalyst support 4-A.

[0038] Step S2: Weigh 34.7g of molybdenum trioxide and 12.5g of basic cobalt carbonate, add deionized water, 5g of phosphoric acid, and 4.5g of citric acid, heat and stir until completely dissolved, cool to room temperature to obtain the impregnation solution. Impregnate 100g of the prepared carrier with the impregnation solution for 60min, let stand for 3h after impregnation, and dry at 150℃ for 4h to obtain the semi-finished product 4-B.

[0039] Step S3: Weigh 5.8g of cobalt nitrate, add deionized water and 7g of citric acid, stir until completely dissolved, and cool to room temperature to obtain an impregnation solution. Spray 100g of the prepared 3-B with the impregnation solution for 30min, let stand for 3h after impregnation, and dry at 80℃ for 4h to obtain catalyst 4-C.

[0040] Example 5

[0041] Step S1: Weigh 60g of alumina powder, add 30g of silica, 2g of boron oxide and 8g of polyvinyl alcohol-sodium polyacrylate cross-linked network hydrogel (molecular weight 20000), knead on a kneader, add 100g of aqueous solution containing 2g of nitric acid dropwise during kneading, extrude into clover-shaped strips with a diameter of 1.3mm, dry at 120℃ for 4h, calcine at 500℃ for 4h to obtain catalyst support 5-A.

[0042] Step S2: Weigh 34.7g of molybdenum trioxide and 16.5g of basic cobalt carbonate, add deionized water, 5g of phosphoric acid, and 4.5g of citric acid, heat and stir until completely dissolved, cool to room temperature to obtain the impregnation solution. Impregnate 100g of the prepared carrier with the impregnation solution for 30min, let stand for 5h after impregnation, and dry at 120℃ for 8h to obtain the finished product 5-C.

[0043] Example 6

[0044] Step S1: Weigh 66g of alumina powder, add 20g of silica, 10g of boron oxide and 4g of polyvinyl alcohol-sodium polyacrylate cross-linked network hydrogel (molecular weight 20000), knead on a kneader, add 100g of aqueous solution containing 2g of nitric acid dropwise during kneading, extrude into clover-shaped strips with a diameter of 1.3mm, dry at 120℃ for 4h, calcine at 500℃ for 4h to obtain catalyst support 6-A.

[0045] Step S2: Weigh 34.7g of molybdenum trioxide and 12.5g of basic cobalt carbonate, add deionized water, 5g of phosphoric acid, and 18g of citric acid, heat and stir until completely dissolved, cool to room temperature to obtain the impregnation solution. Impregnate 100g of the prepared carrier with the impregnation solution for 60min, let stand for 3h after impregnation, and dry at 170℃ for 4h to obtain the finished product 6-C.

[0046] Example 7

[0047] Step S1: Weigh 64g of alumina powder, add 20g of silica, 10g of boron oxide and 6g of polypropylene cross-linked network hydrogel (molecular weight 4000), knead on a kneader, add 100g of aqueous solution containing 2g of nitric acid dropwise during kneading, extrude into clover-shaped strips with a diameter of 1.3mm, dry at 120℃ for 4h, calcine at 500℃ for 4h to obtain catalyst support 7-A.

[0048] Step S2: Weigh 34.7g of molybdenum trioxide and 12.5g of basic cobalt carbonate, add deionized water, 5g of phosphoric acid, and 6g of pentaerythritol, heat and stir until completely dissolved, cool to room temperature to obtain the impregnation solution. Impregnate 100g of the prepared carrier with the impregnation solution for 60min, let stand for 3h after impregnation, and dry at 150℃ for 4h to obtain the finished product 7-C.

[0049] Example 8

[0050] Step S1: Weigh 64g of alumina powder, add 20g of silica, 10g of boron oxide and 6g of polyethylene glycol cross-linked network hydrogel (molecular weight 8000), knead on a kneader, add 100g of aqueous solution containing 2g of nitric acid dropwise during kneading, extrude into clover-shaped strips with a diameter of 1.3mm, dry at 120℃ for 4h, calcine at 500℃ for 4h to obtain catalyst support 8-A.

[0051] Step S2: Weigh 34.7g of molybdenum trioxide and 16.5g of basic cobalt carbonate, add deionized water, 5g of phosphoric acid, and 4.5g of ascorbic acid, heat and stir until completely dissolved, cool to room temperature to obtain the impregnation solution. Impregnate 100g of the prepared carrier with the impregnation solution for 30min, let stand for 5h after impregnation, and dry at 120℃ for 8h to obtain the finished product 8-C.

[0052] Comparative Example 1

[0053] Step S1: Weigh 64g of alumina powder, add 20g of silicon dioxide and 10g of boron oxide, and knead them in a kneader. During the kneading process, add 100g of an aqueous solution containing 2g of nitric acid. Extrude the mixture into a clover shape with a diameter of 1.3mm, dry it at 120℃ for 4h, and calcine it at 500℃ for 4h to obtain catalyst support A.

[0054] Step S2: Weigh 34.7g of molybdenum trioxide and 12.5g of basic cobalt carbonate, add deionized water and 5g of phosphoric acid, heat and stir until completely dissolved, cool to room temperature to obtain an impregnation solution. Impregnate 100g of the prepared support with the impregnation solution for 60min, let stand for 3h after impregnation, and dry at 150℃ for 4h to obtain catalyst D.

[0055] To make the function of the heavy distillate oil hydrorefining sulfide catalyst of the present invention clearer, the concentration distribution of active metals in the above-mentioned examples and comparative examples of heavy distillate oil hydrorefining sulfide catalysts is analyzed below.

[0056] Figure 1 This is a distribution diagram of the active metal concentration in catalyst 2-C; Figure 2 This is a distribution diagram of the active metal concentration of catalyst D. The horizontal axis represents the distance between a certain location on the catalyst and the catalyst center, with 0 representing the catalyst center and 1 representing the outer surface of the catalyst. The vertical axis represents the Co / Mo atomic ratio of the active metal at that location.

[0057] The catalytic activity of the heavy distillate hydrorefining sulfide-state catalysts used in the examples and comparative examples was evaluated. The evaluation feedstock was a mixture of straight-run diesel, catalytic diesel, and coking diesel, with a density of 820 kg / m³. 3 The sulfur content was 1200 ug / g, and the nitrogen content was 900 ug / g. The catalyst loading was 100 mL, the feed rate of the mixed diesel was 100 mL / h, the hydrogen-to-oil ratio was 1000, the reactor temperature was 400℃, and samples were taken for analysis after stabilization for 24 h. The evaluation results are shown in Table 1.

[0058] Table 1. Catalyst activity evaluation data

[0059]

[0060] As can be seen from Table 1, compared with Examples 1-4 and Comparative Example 1, no metal complexing agent was added in Comparative Example 1.

[0061] The main difference between Example 3 and Example 2 is that the amount of complexing agent added in step S2 is different, resulting in a higher Co concentration on the surface than inside after impregnation in step 1.

[0062] The main difference between Example 4 and Example 2 is the addition of step S3, which involves impregnating the surface with a Co impregnation solution. This results in a higher Co concentration on the surface compared to the interior, making the uneven distribution of cobalt more pronounced.

[0063] In summary, the present invention provides a sulfide-containing catalyst for the hydrorefining of heavy distillate oil and its preparation method. This method involves impregnating active metals molybdenum and cobalt to ensure uniform distribution of molybdenum on a support. An organic complexing agent is added to adjust the impregnation rate of nickel and cobalt, and the impregnation time and drying rate are controlled to achieve an eggshell-shaped distribution of nickel and cobalt on the support. The resulting sulfide-containing catalyst for the hydrorefining of heavy distillate oil has a large average pore size and high hydrodesulfurization and denitrification activity.

[0064] Of course, the present invention may have other various embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art can make various corresponding changes and modifications according to the present invention, but these corresponding changes and modifications should all fall within the protection scope of the claims of the present invention.

Claims

1. A catalyst for the hydrorefining of heavy distillate oil, characterized in that, The device includes a carrier and an active component. The carrier has a network structure with through-pores. The active component includes cobalt oxide, molybdenum oxide, and / or tungsten oxide. The concentration of cobalt oxide decreases from the surface to the interior of the carrier, and the concentration of molybdenum oxide and / or tungsten oxide is uniformly distributed on the carrier. A cross-linking polymer is added during the preparation of the carrier, and then the cross-linking polymer is ablated by calcination to obtain a network structure with through-pores. The crosslinked polymer is one or more of polyvinyl alcohol-sodium polyacrylate, polyethylene glycol, and polypropylene glycol.

2. The heavy distillate oil hydrorefining catalyst according to claim 1, characterized in that, Based on the catalyst weight of 100%, the cobalt oxide content is 2-10%, and the molybdenum oxide and / or tungsten oxide content is 18-30%.

3. The heavy distillate oil hydrorefining catalyst according to claim 1, characterized in that, The carrier includes alumina and / or silicon dioxide.

4. The heavy distillate oil hydrorefining catalyst according to claim 1, characterized in that, The amount of the cross-linked polymer added is 4 to 8 wt% of the total amount of the carrier raw material.

5. The heavy distillate oil hydrorefining catalyst according to claim 1, characterized in that, Boron oxide is also added during the preparation of the carrier, and the amount of boron oxide added is 2 to 10 wt% of the total amount of carrier raw materials.

6. The method for preparing the heavy distillate oil hydrorefining catalyst according to any one of claims 1 to 5, characterized in that, Includes the following steps: S1, mix the carrier raw materials, add acid solution, and then extrude, shape, dry and calcine to obtain a carrier with a network of interconnected pores; S2, mix the active component precursor, water, organic complexing agent and phosphorus-containing precursor to prepare an impregnation solution, impregnate the support, and then dry to obtain the finished catalyst.

7. The method for preparing the heavy distillate oil hydrorefining catalyst according to claim 6, characterized in that, The organic complexing agent is an organic acid and / or a polyol, wherein the organic acid is one or more of citric acid, oxalic acid and ascorbic acid, and the polyol is pentaerythritol and / or diethylene glycol.

8. The method for preparing the heavy distillate oil hydrorefining catalyst according to claim 6, characterized in that, In step S2, the soaking time is 30-60 minutes, the drying temperature is 120-170℃, and the drying time is 4-8 hours.

9. The method for preparing the heavy distillate oil hydrorefining catalyst according to claim 6, characterized in that, The acid solution mentioned in step S1 is a nitric acid solution or a phosphoric acid solution.

Citation Information

Patent Citations

  • Hydrogenation catalyst with active metal component concentration in gradient increasing distribution and preparation method thereof

    CN101927169B

  • A kind of hydrotreating catalyst, its preparation method and its application

    CN103801314B

  • Hydrotreatment catalyst and preparation method thereof

    CN104588029A

  • Preparation method of alumina carrier

    CN114653351A

  • Method of preparing catalyst for hydrogenation of hydrocarbon oil

    US5232888A