A method for establishing a continuous dynamic recrystallization model coupled with a macro-meso finite element model, crystal plasticity and cellular automaton
By combining macro-micro finite element models and cellular automata, and considering the influence of second-phase particles, a continuous dynamic recrystallization model was established, which solved the problem of inaccurate prediction in existing technologies and achieved accurate simulation and interpretation of recrystallization behavior.
Patent Information
- Application Number
- CN202410304209.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-18
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-03-18
AI Technical Summary
Existing technologies struggle to accurately predict the continuous dynamic recrystallization behavior of materials in terms of modeling, especially failing to consider the influence of second-phase particles on dislocation density and subgrain orientation, resulting in inaccurate predictions.
By combining macro-micro finite element models, crystal plasticity, and cellular automata, a continuous dynamic recrystallization model is established by acquiring SEM and EBSD image parameters of the material, taking into account the influence of second-phase particles. This includes establishing a thermally compressible geometric model, assigning material parameters, mesh generation, and a cellular automata model to simulate the formation and growth process of recrystallized grains.
It achieves accurate simulation and prediction of the continuous dynamic recrystallization behavior of materials, improves the accuracy of the model, can reasonably simulate the formation of recrystallized grains and explain their internal formation principle, and is consistent with experimental results.
Smart Images

Figure CN118248258B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of computational materials science, specifically to a method for establishing a continuous dynamic recrystallization model that couples macro-micro finite element models, crystal plasticity, and cellular automata. Background Technology
[0002] Recrystallization is a form of material crystallization process. According to the process in which it occurs, it is divided into static recrystallization (SRX) and dynamic recrystallization (DRX). Static recrystallization occurs during annealing, while dynamic recrystallization occurs during hot deformation.
[0003] Continuous dynamic recrystallization occurs during hot deformation when subgrain boundaries continuously absorb dislocations, causing the orientation difference angle to increase and leading to subgrain rotation. Ultimately, the subgrain transitions from small-angle to large-angle grain boundaries, meaning the subgrain becomes a true grain. Therefore, the continuous dynamic recrystallization model needs to consider the evolution of dislocation density and subgrain orientation. In addition, during deformation, second-phase particles in the material cause dislocation multiplication and subgrain orientation rotation; therefore, the continuous dynamic recrystallization model also needs to consider the influence of second-phase particles on dislocation density and subgrain orientation.
[0004] Classic image analysis methods include electron backscatter diffraction (EBSD), a technique that uses diffracted electron beams to identify the crystallographic orientation of a sample. Mounted in a scanning electron microscope (SEM), it allows direct observation of recrystallized grains, but its accuracy is limited due to resolution constraints.
[0005] Existing technologies primarily rely on internal variable models for modeling. However, these models involve multiple material parameters, making accurate identification difficult and computationally intensive, thus failing to predict the true evolution of recrystallized grain morphology during recrystallization. Furthermore, they do not consider the continuous recrystallization of second-phase particles within the material, resulting in inaccurate predictions of the material's continuous dynamic recrystallization behavior. Summary of the Invention
[0006] The purpose of this invention is to provide a method for establishing a continuous dynamic recrystallization model that couples macro-micro finite element models, crystal plasticity, and cellular automata, comprising the following steps:
[0007] 1) Obtain SEM and EBSD images of the workpiece material before deformation, and extract the geometric parameters from the SEM and EBSD images.
[0008] 2) Establish a macroscopic finite element model.
[0009] 3) Based on the macroscopic finite element model and the geometric parameters in the SEM and EBSD images, a microscopic finite element model is established.
[0010] 4) Extract the Euler angles and shear strain rate from the mesoscopic finite element model.
[0011] 5) Based on Euler angles and shear strain rate, the corresponding orientation matrix and dislocation density are calculated.
[0012] 6) Based on the orientation matrix and dislocation density, a cellular automata model is established.
[0013] 7) Return to step 4) and perform the calculation for the next incremental step until the prediction of the dynamic recrystallization evolution coupling response is completed and the continuous recrystallization model is established.
[0014] Furthermore, the geometric parameters in the SEM image and EBSD image include the size of the EBSD image, the size of the micro-region in the EBSD image, the dislocation density and Euler angle of each micro-region in the EBSD image, the pixel position of the center of the second phase particle in the SEM image, and the size of the second phase particle in the SEM image.
[0015] Furthermore, the steps for establishing the macroscopic finite element model include:
[0016] 2.1) Establish a thermal compression geometric model based on the actual dimensions of the workpiece.
[0017] 2.2) Assign stress-strain curves, elastic parameters, and thermophysical parameters to the thermal compression geometric model.
[0018] 2.3) Set load boundary conditions according to the actual load and mold conditions.
[0019] 2.4) The thermal compression geometric model is meshed using a hexahedral mesh.
[0020] Furthermore, the step of establishing a mesoscopic finite element model based on the macroscopic finite element model and the geometric parameters in the SEM and EBSD images includes:
[0021] 3.1) By merging the matrix geometric model and the second-phase particle geometric model, a representative volume element geometric model containing the second-phase particles is established.
[0022] The matrix geometric model is established using the length, width, and micro-region size distribution of the EBSD image as its length, width, and height.
[0023] The geometric model of the second phase particles is established based on the size of the second phase particles in the SEM image, at the position of the center of the second phase particles.
[0024] 3.2) Mesh the geometric model of the representative volume element containing the second phase particles.
[0025] 3.3) Assign material parameters to the geometric model of the representative volume element containing the second-phase particles.
[0026] 3.4) Set the calculated displacement in the numerical simulation results of the macroscopic finite element model as the load boundary condition of the microscopic finite element model.
[0027] Furthermore, the material parameters include elastic parameters, plastic parameters, thermophysical parameters, and Euler angles.
[0028] Furthermore, the step of assigning material parameters to the geometric model of the representative volume element containing the second-phase particles is as follows:
[0029] 3.3.1) Number each mesh in the geometric model of the representative volume element containing the second-phase particles.
[0030] 3.3.2) Based on the geometric positions of the matrix and the second-phase particles, determine whether each grid in the geometric model of the representative volume element containing the second-phase particles corresponds to the matrix. If yes, the grid number remains unchanged; otherwise, the grid number is set to 0.
[0031] 3.3.3) Assign the material parameters of the second phase particles to the mesh numbered 0, and assign the material parameters of the matrix to the meshes not numbered 0.
[0032] Furthermore, the orientation matrix is shown below:
[0033]
[0034] In the formula, Q is the orientation matrix. φ1, φ2, and Φ all represent Euler angles.
[0035] Furthermore, the dislocation density is as follows:
[0036]
[0037] In the formula, ρ represents the dislocation density of each grid cell. a represents the slip system number. N s This represents the number of slip systems. ρ a Let represent the dislocation density of the slip system a.
[0038] Wherein, the dislocation density ρ of the slip system a a The result is obtained by formula (3):
[0039]
[0040] In the formula, It is the dislocation density index of the slip system a. It is the shear strain rate of slip system a. It is a coefficient related to work hardening.
[0041] Among them, the coefficients related to dynamic response As shown below:
[0042]
[0043] In the formula, n1 and n2 both represent material parameters, R is the ideal gas parameter, and Q is the material parameter. act It is the deformation activation energy, and T is the deformation temperature.
[0044] Furthermore, the steps for establishing the cellular automata model include:
[0045] 6.1) Construct a recrystallization grain nucleation model by using the orientation difference angle of subgrains.
[0046] If the orientation difference angle between the current subcrystal and any adjacent subcrystal is greater than x degrees, then the current subcrystal is a recrystallized grain, where x is a positive number.
[0047] The orientation difference angle between the two adjacent subgrains is shown below:
[0048] θ = arccos(0.5(q) 11 +q 22 +q 33 (5)
[0049] In the formula, θ is the orientation difference angle between two adjacent subcrystals. 11 q 22 q 33 The orientation difference matrix Q of each of the two adjacent subcrystals 12 The diagonal elements.
[0050] Among them, the orientation difference matrix Q of two adjacent subcrystals 12 As shown below:
[0051]
[0052] In the formula, Q2 is the orientation matrix of adjacent subgrains, [Q1] -1 q is the inverse of the orientation matrix of the current subgrain. 12 q 13 q 21 q 23 q 31 q 32 The orientation difference matrix Q of each of the two adjacent subgrains 12 Element.
[0053] 6.2) Construct a recrystallization grain growth model.
[0054] The conditions for the growth of the recrystallized grains are as follows:
[0055] νΔt≥L cell (7)
[0056] In the formula, L cell It is the length of the cell. Δt is the increment per unit time.
[0057] The grain boundary growth rate ν is shown below:
[0058] ν=MP (8)
[0059] The grain boundary mobility M is shown below:
[0060]
[0061] In the formula, δ is the grain boundary thickness, and D... ob It is the grain boundary diffusion coefficient at absolute zero, K is the Boltzmann constant, b is the Borgs vector, and Q is the absolute zero temperature. b It is the diffusion activation energy. R is the ideal gas parameter, and T is the deformation temperature.
[0062] The driving force P is shown below:
[0063] P = P1 + P2 + P3 (10)
[0064] The driving force P1 caused by surface energy is shown below:
[0065]
[0066] In the formula, ρ m ρ d These are the dislocation densities of the matrix grains and recrystallized grains, respectively, and μ is the shear modulus of the material.
[0067] The drag force P2 caused by volume energy is shown below:
[0068]
[0069] In the formula, r d It is the radius of the dynamically recrystallized grain.
[0070] The high-angle grain boundary energy γ is shown below:
[0071]
[0072] In the formula, υ1 is Poisson's ratio. θ m It is the orientation difference angle of a large-angle grain boundary.
[0073] The Zener resistance P3 caused by the second-phase particles is shown below:
[0074]
[0075] In the formula, r s f s These are the radius and percentage of the second-phase particles, respectively.
[0076] Furthermore, the step of establishing the continuous recrystallization model includes:
[0077] 7.1) Initialize the cellular automaton model and define the unit time increment as Δt, with the current time t = 1.
[0078] 7.2) Based on the correspondence between the mesh positions in the mesoscopic finite element model and the cell positions in the cellular automaton model, the cells in the cellular automaton model are numbered, and the deformation temperature, orientation matrix, and dislocation density in the mesoscopic finite element model at the current time t are assigned to the cells.
[0079] 7.3) Scan the cell space and define the color display values of grain boundary cells, recrystallization cells, second phase particle cells, and intragranular cells as 0, 0.5, 1, and 0.75, respectively.
[0080] The recrystallization cell is cell numbered 0.5.
[0081] If the orientation difference angle between two adjacent subgrains is greater than the orientation difference angle θ of a large-angle grain boundary m If so, the current cell number is 0.5.
[0082] The second phase particle cell is cell numbered 0.
[0083] The grain boundary cell is defined as follows: apart from recrystallization cells and second-phase particle cells, if the orientation difference angle between the current cell and any adjacent cell is greater than x degrees, then the current cell becomes a grain boundary cell, where x is a positive number.
[0084] The intragranular cells are the cells remaining excluding grain boundary cells, recrystallization cells, and second-phase particle cells.
[0085] 7.4) Calculate the orientation difference angle of each cell except for the second phase particle cells and grain boundary cells, and determine whether the orientation difference angle of each cell is greater than x degrees. If so, the cell nucleation is successful.
[0086] For cells that have successfully formed nuclei, change the current state of the cell and randomly assign a new orientation different from that of the adjacent cells. Increase the recrystallization count by 1, reduce the dislocation density to the initial value, and update the cell number to 0.5.
[0087] 7.5) Determine whether each cell other than the second-phase grain cell has met the grain growth conditions. If so, the current cell state changes and the dislocation density, recrystallization size, orientation and color display value of the current cell are consistent with the target cell.
[0088] The target cell is the neighboring cell of the current cell.
[0089] 7.6) Determine if t has reached the preset total time step T. If yes, output the recrystallization percentage, recrystallized grain size, and microstructure image. If no, return to step 7.2).
[0090] The technical effect of this invention is beyond doubt. The continuous dynamic recrystallization model established by this invention through coupling macroscopic finite element model, mesoscopic finite element model, crystal plasticity model and cellular automata model can accurately simulate actual recrystallization behavior.
[0091] The continuous recrystallization model considering second-phase particles developed in this invention can accurately predict the continuous dynamic recrystallization behavior of materials, and the continuous recrystallization model considering second-phase particles has better accuracy compared with the continuous recrystallization model that does not consider second-phase particles.
[0092] The subgrain rotation nucleation theory provided by this invention is applied to the developed continuous recrystallization model. This model can not only reasonably simulate the formation of recrystallized grains, but also explain the formation principle of different recrystallized grains inside the grain.
[0093] The continuous recrystallization model developed in this invention has an initial microstructure consistent with the experiment, and can accurately and realistically reflect the morphological evolution of recrystallized grains during the recrystallization process. Attached Figure Description
[0094] Figure 1 The algorithm flow for the continuous recrystallization model;
[0095] Figure 2 The stress-strain curve of 2219 aluminum alloy is shown. Detailed Implementation
[0096] The present invention will be further described below with reference to embodiments, but it should not be construed that the scope of the present invention is limited to the following embodiments. Various substitutions and modifications made based on ordinary technical knowledge and common practices in the art without departing from the above-described technical concept of the present invention should be included within the scope of protection of the present invention.
[0097] Example 1:
[0098] See Figures 1 to 2 A method for establishing a continuous dynamic recrystallization model that couples macro-micro finite element models, crystal plasticity, and cellular automata includes the following steps:
[0099] 1) Obtain SEM and EBSD images of the workpiece material before deformation, and extract the geometric parameters from the SEM and EBSD images.
[0100] 2) Establish a macroscopic finite element model.
[0101] 3) Based on the macroscopic finite element model and the geometric parameters in the SEM and EBSD images, a microscopic finite element model is established.
[0102] 4) Extract the Euler angles and shear strain rate from the mesoscopic finite element model.
[0103] 5) Based on Euler angles and shear strain rate, the corresponding orientation matrix and dislocation density are calculated.
[0104] 6) Based on the orientation matrix and dislocation density, a cellular automata model is established.
[0105] 7) Return to step 4) and perform the calculation for the next incremental step until the prediction of the dynamic recrystallization evolution coupling response is completed and the continuous recrystallization model is established.
[0106] Example 2:
[0107] A method for establishing a continuous dynamic recrystallization model coupled with macro-micro finite element model, crystal plasticity and cellular automata, the main technical contents of which are described in Example 1. Further, the geometric parameters in the SEM image and EBSD image include the size of the EBSD image, the size of the micro-region in the EBSD image, the dislocation density and Euler angle of each micro-region in the EBSD image, the pixel position of the center of the second phase particle in the SEM image, and the size of the second phase particle in the SEM image.
[0108] Example 3:
[0109] A method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata, the main technical contents of which are described in any one of Examples 1 to 2. Further, the steps for establishing the macro-finite element model include:
[0110] 2.1) Establish a thermal compression geometric model based on the actual dimensions of the workpiece.
[0111] 2.2) Assign stress-strain curves, elastic parameters, and thermophysical parameters to the thermal compression geometric model.
[0112] 2.3) Set load boundary conditions according to the actual load and mold conditions.
[0113] 2.4) The thermal compression geometric model is meshed using a hexahedral mesh.
[0114] Example 4:
[0115] A method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata, the main technical contents of which are described in any one of Examples 1 to 3. Further, the steps for establishing the micro finite element model based on the macro-finite element model and geometric parameters in SEM and EBSD images include:
[0116] 3.1) By merging the matrix geometric model and the second-phase particle geometric model, a representative volume element geometric model containing the second-phase particles is established.
[0117] The matrix geometric model is established using the length, width, and micro-region size distribution of the EBSD image as its length, width, and height.
[0118] The geometric model of the second phase particles is established based on the size of the second phase particles in the SEM image, at the position of the center of the second phase particles.
[0119] 3.2) Mesh the geometric model of the representative volume element containing the second phase particles.
[0120] 3.3) Assign material parameters to the geometric model of the representative volume element containing the second-phase particles.
[0121] 3.4) Set the calculated displacement in the numerical simulation results of the macroscopic finite element model as the load boundary condition of the microscopic finite element model.
[0122] Example 5:
[0123] A method for establishing a continuous dynamic recrystallization model that couples macro-micro finite element model, crystal plasticity and cellular automata, the main technical contents of which are described in any one of Examples 1 to 4. Further, the material parameters include elastic parameters, plastic parameters, thermophysical parameters and Euler angles.
[0124] Example 6:
[0125] A method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata, the main technical contents of which are described in any one of Examples 1 to 5. Further, the step of assigning material parameters to the geometric model of the representative volume element containing second-phase particles is as follows:
[0126] 3.3.1) Number each mesh in the geometric model of the representative volume element containing the second-phase particles.
[0127] 3.3.2) Based on the geometric positions of the matrix and the second-phase particles, determine whether each grid in the geometric model of the representative volume element containing the second-phase particles corresponds to the matrix. If yes, the grid number remains unchanged; otherwise, the grid number is set to 0.
[0128] 3.3.3) Assign the material parameters of the second phase particles to the mesh numbered 0, and assign the material parameters of the matrix to the meshes not numbered 0.
[0129] Example 7:
[0130] A method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata, the main technical contents of which are described in any one of Examples 1 to 6. Further, the orientation matrix is shown below:
[0131]
[0132] In the formula, Q is the orientation matrix. φ1, φ2, and Φ all represent Euler angles.
[0133] Example 8:
[0134] A method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata, the main technical contents of which are described in any one of Examples 1 to 7. Further, the dislocation density is as follows:
[0135]
[0136] In the formula, ρ represents the dislocation density of each grid cell. a represents the slip system number. N s This represents the number of slip systems. ρ a Let represent the dislocation density of the slip system a.
[0137] Wherein, the dislocation density ρ of the slip system a a The result is obtained by formula (3):
[0138]
[0139] In the formula, It is the dislocation density index of the slip system a. It is the shear strain rate of slip system a. It is a coefficient related to work hardening.
[0140] Among them, the coefficients related to dynamic response As shown below:
[0141]
[0142] In the formula, n1 and n2 both represent material parameters, R is the ideal gas parameter, and Q is the material parameter. act It is the deformation activation energy, and T is the deformation temperature.
[0143] Example 9:
[0144] A method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata, the main technical contents of which are described in any one of Examples 1 to 8, further comprising the following steps for establishing the cellular automata model:
[0145] 6.1) Construct a recrystallization grain nucleation model by using the orientation difference angle of subgrains.
[0146] If the orientation difference angle between the current subcrystal and any adjacent subcrystal is greater than x degrees, then the current subcrystal is a recrystallized grain, where x is a positive number.
[0147] The orientation difference angle between the two adjacent subgrains is shown below:
[0148] θ = arccos(0.5(q) 11 +q 22 +q 33 (5)
[0149] In the formula, θ is the orientation difference angle between two adjacent subcrystals. 11 q 22 q 33 The orientation difference matrix Q of each of the two adjacent subgrains 12 The diagonal elements.
[0150] Among them, the orientation difference matrix Q of two adjacent subcrystals 12 As shown below:
[0151]
[0152] In the formula, Q2 is the orientation matrix of adjacent subgrains, [Q1] -1 q is the inverse of the orientation matrix of the current subgrain. 12 q 13 q 21 q 23 q 31 q 32 The orientation difference matrix Q of each of the two adjacent subgrains 12 Element.
[0153] 6.2) Construct a recrystallization grain growth model.
[0154] The conditions for the growth of the recrystallized grains are as follows:
[0155] νΔt≥L cell (7)
[0156] In the formula, L cell It is the length of the cell. Δt is the increment per unit time.
[0157] The grain boundary growth rate ν is shown below:
[0158] ν=MP (8)
[0159] The grain boundary mobility M is shown below:
[0160]
[0161] In the formula, δ is the grain boundary thickness, and D... ob It is the grain boundary diffusion coefficient at absolute zero, K is the Boltzmann constant, b is the Borgs vector, and Q is the absolute zero temperature. b It is the diffusion activation energy. R is the ideal gas parameter, and T is the deformation temperature.
[0162] The driving force P is shown below:
[0163] P = P1 + P2 + P3 (10)
[0164] The driving force P1 caused by surface energy is shown below:
[0165]
[0166] In the formula, ρ m ρ d These are the dislocation densities of the matrix grains and recrystallized grains, respectively, and μ is the shear modulus of the material.
[0167] The drag force P2 caused by volume energy is shown below:
[0168]
[0169] In the formula, r d It is the radius of the dynamically recrystallized grain.
[0170] The high-angle grain boundary energy γ is shown below:
[0171]
[0172] In the formula, υ1 is Poisson's ratio. θ m It is the orientation difference angle of a large-angle grain boundary.
[0173] The Zener resistance P3 caused by the second-phase particles is shown below:
[0174]
[0175] In the formula, r s f s These are the radius and percentage of the second-phase particles, respectively.
[0176] Example 10:
[0177] A method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata, the main technical contents of which are described in any one of Examples 1 to 9, further comprising the following steps for establishing the continuous recrystallization model:
[0178] 7.1) Initialize the cellular automaton model and define the unit time increment as Δt, with the current time t = 1.
[0179] 7.2) Based on the correspondence between the mesh positions in the mesoscopic finite element model and the cell positions in the cellular automaton model, the cells in the cellular automaton model are numbered, and the deformation temperature, orientation matrix, and dislocation density in the mesoscopic finite element model at the current time t are assigned to the cells.
[0180] 7.3) Scan the cell space and define the color display values of grain boundary cells, recrystallization cells, second phase particle cells, and intragranular cells as 0, 0.5, 1, and 0.75, respectively.
[0181] The recrystallization cell is cell numbered 0.5.
[0182] If the orientation difference angle between two adjacent subgrains is greater than the orientation difference angle θ of a large-angle grain boundary m If so, the current cell number is 0.5.
[0183] The second phase particle cell is cell numbered 0.
[0184] The grain boundary cell is defined as follows: apart from recrystallization cells and second-phase particle cells, if the orientation difference angle between the current cell and any adjacent cell is greater than x degrees, then the current cell becomes a grain boundary cell, where x is a positive number.
[0185] The intragranular cells are the cells remaining excluding grain boundary cells, recrystallization cells, and second-phase particle cells.
[0186] 7.4) Calculate the orientation difference angle of each cell except for the second phase particle cells and grain boundary cells, and determine whether the orientation difference angle of each cell is greater than x degrees. If so, the cell nucleation is successful.
[0187] For cells that have successfully formed nuclei, change the current state of the cell and randomly assign a new orientation different from that of the adjacent cells. Increase the recrystallization count by 1, reduce the dislocation density to the initial value, and update the cell number to 0.5.
[0188] 7.5) Determine whether each cell other than the second-phase grain cell has met the grain growth conditions. If so, the current cell state changes and the dislocation density, recrystallization size, orientation and color display value of the current cell are consistent with the target cell.
[0189] The target cell is the neighboring cell of the current cell.
[0190] 7.6) Determine if t has reached the preset total time step T. If yes, output the recrystallization percentage, recrystallized grain size, and microstructure image. If no, return to step 7.2).
[0191] Example 11:
[0192] See Figures 1 to 2 A method for establishing a continuous dynamic recrystallization model that couples macro-micro finite element models, crystal plasticity, and cellular automata includes the following steps:
[0193] 1) Initial microstructure imaging: SEM and EBSD images of the workpiece material structure before deformation were obtained by scanning electron microscopy, and geometric parameters were extracted from the SEM and EBSD images.
[0194] The observed workpiece is made of aluminum alloy.
[0195] The SEM image and the EBSD image are kept to the same size.
[0196] 2) Establish a macroscopic finite element model.
[0197] A macroscopic finite element model is established in ABAQUS software. This macroscopic finite element model includes the establishment of a hot-compressive geometry model, assignment of material parameters, setting of boundary conditions, and mesh generation.
[0198] 3) Based on the macroscopic finite element model and the geometric parameters in the SEM and EBSD images, a microscopic finite element model is established, and an RVE finite element model is established in ABAQUS software.
[0199] 4) Extract the Euler angles and shear strain rate from the mesoscopic finite element model.
[0200] To obtain the Euler angles of each mesh in the mesoscale finite element model, DAMASK was used as the UMAT implementation of ABAQUS to realize the crystal plasticity model as the material constitutive model in the mesoscale finite element model. Based on the mesoscale numerical simulation results, the Euler angles and shear strain rates of each mesh at each time increment step were extracted.
[0201] 5) Based on Euler angles and shear strain rate, the corresponding orientation matrix and dislocation density are calculated.
[0202] 6) In order to simulate the evolution of microstructure during hot deformation, the nucleation and growth rules of recrystallized grains need to be defined. Based on the orientation matrix and dislocation density, a cellular automata model is established.
[0203] 7) Return to step 4) and perform the calculation for the next incremental step until the prediction of the dynamic recrystallization evolution coupling response is completed and the continuous recrystallization model is established.
[0204] Example 12:
[0205] A method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata is described in Example 11. Further, the geometric parameters in the SEM image and EBSD image include the size of the EBSD image, the size of the micro-region in the EBSD image, the dislocation density and Euler angle of each micro-region in the EBSD image, the pixel position of the center of the second phase particle in the SEM image, and the size of the second phase particle in the SEM image.
[0206] The dimensions of the EBSD image, the dimensions of small regions within the EBSD image, and the dislocation density and Euler angles of each small region can be extracted using OIM software. The pixel locations of the second-phase particle centers in the SEM image are identified using the PIL toolkit in Python, and the dimensions of the second-phase particles in the SEM image are extracted using Image-Pro Plus software.
[0207] The tiny areas in an EBSD image are determined by the parameters of the captured EBSD image (capture stride).
[0208] The volume fraction of second-phase particles varies considerably among different materials. This volume fraction of second-phase particles can be obtained by statistically analyzing SEM images of the material.
[0209] Example 13:
[0210] A method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata, the main technical contents of which are described in any one of Examples 11 to 12. Further, the steps for establishing the macro-finite element model include:
[0211] 2.1) Establish a thermal compression geometric model based on the actual dimensions of the workpiece.
[0212] 2.2) Assign stress-strain curves, elastic parameters, and thermophysical parameters to the thermal compression geometric model.
[0213] 2.3) Set load boundary conditions according to the actual load and mold conditions.
[0214] Boundary condition settings are related to the mold. For example, the friction between the mold and the workpiece, and the mold's moving speed.
[0215] 2.4) The thermally compressed geometric model is meshed using a hexahedral mesh, and the size of the mesh is consistent with the size of the small region in the EBSD image.
[0216] Example 14:
[0217] A method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata, the main technical contents of which are described in any one of Examples 11 to 13. Further, the step of establishing the micro finite element model based on the macro-finite element model and geometric parameters in SEM and EBSD images includes:
[0218] 3.1) By merging the matrix geometric model and the second-phase particle geometric model, a representative volume element (RVE) geometric model containing second-phase particles is established.
[0219] The matrix geometric model is established using the length, width, and micro-region size distribution of the EBSD image as its length, width, and height.
[0220] The geometric model of the second phase particles is established based on the size of the second phase particles in the SEM image, at the position of the center of the second phase particles.
[0221] 3.2) Mesh the representative volume element geometric model containing second-phase particles, wherein the size of the mesh is consistent with the size of the small region in the EBSD image.
[0222] 3.3) Assign material parameters to the geometric model of the representative volume element containing the second-phase particles.
[0223] 3.4) Using the SUBMODEL module in ABAQUS, the calculated displacement in the numerical simulation results of the macroscopic finite element model is set as the load boundary condition of the microscopic finite element model. The key to setting this boundary condition is that the position of the microscopic finite element model is consistent with the position of the macroscopic finite element model.
[0224] Example 15:
[0225] A method for establishing a continuous dynamic recrystallization model that couples macro-micro finite element model, crystal plasticity and cellular automata, the main technical contents of which are described in any one of Examples 11 to 14. Further, the material parameters include elastic parameters, plastic parameters, thermophysical parameters and Euler angles.
[0226] Example 16:
[0227] A method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata, the main technical contents of which are described in any one of Examples 11 to 15, further comprising the following steps for assigning material parameters to the geometric model of the representative volume element containing second-phase particles:
[0228] 3.3.1) Number each mesh in the geometric model of the representative volume element containing the second-phase particles.
[0229] 3.3.2) Based on the geometric positions of the matrix and the second-phase particles, determine whether each grid in the geometric model of the representative volume element containing the second-phase particles corresponds to the matrix. If yes, the grid number remains unchanged; otherwise, the grid number is set to 0.
[0230] 3.3.3) Assign the material parameters of the second phase particles to the mesh numbered 0, and assign the material parameters of the matrix to the meshes not numbered 0.
[0231] Example 17:
[0232] A method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata is provided. The main technical details are described in any one of Examples 11 to 16. Further, the extracted Euler angles are converted into an orientation matrix based on the relationship between Euler angles and the orientation matrix, as shown below:
[0233]
[0234] In the formula, Q is the orientation matrix. φ1, φ2, and Φ all represent Euler angles.
[0235] Example 18:
[0236] A method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata is provided. The main technical details are described in any one of Examples 11 to 17. Further, based on the modified Kocks and Mecking model and the extracted shear strain rate, the dislocation density corresponding to each mesh is calculated. The dislocation density is shown below:
[0237]
[0238] In the formula, ρ represents the dislocation density of each grid cell. a represents the slip system number. N s This represents the number of slip systems. ρ a Let represent the dislocation density of the slip system a.
[0239] Wherein, the dislocation density ρ of the slip system a a The result is obtained by formula (3):
[0240]
[0241] In the formula, It is the dislocation density index of the slip system a. It is the shear strain rate of slip system a. It is a coefficient related to work hardening.
[0242] Among them, the coefficients related to dynamic response As shown below:
[0243]
[0244] In the formula, n1 and n1 both represent material parameters, R is the ideal gas parameter, and Q is the material parameter. act It is the deformation activation energy, and T is the deformation temperature.
[0245] Example 19:
[0246] A method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata, the main technical contents of which are described in any one of Examples 11 to 18, further comprising the following steps for establishing the cellular automata model:
[0247] 6.1) Construct a recrystallization grain nucleation model by using the orientation difference angle of subgrains.
[0248] For continuous dynamic recrystallization, the large-angle grain boundaries of new grains mainly arise from the gradual increase in the orientation difference angle of the subgrains. Therefore, the nucleation rule can be determined by the orientation difference angle of the subgrains. If the orientation difference angle between the current subgrain and any adjacent subgrain is greater than 15 degrees, then the current subgrain is a recrystallized grain.
[0249] The orientation difference angle between the two adjacent subgrains is shown below:
[0250] θ = arccos(0.5(q) 11 +q 22 +q 33 (5)
[0251] In the formula, θ is the orientation difference angle between two adjacent subcrystals. 11 q 22 q 33 The orientation difference matrix Q of each of the two adjacent subgrains 12 The diagonal elements. The calculation of this orientation difference serves not only as a condition for recrystallization grain nucleation but also as a basis for defining large-angle grain boundary cells.
[0252] Among them, the orientation difference matrix Q of two adjacent subcrystals 12 As shown below:
[0253]
[0254] In the formula, Q2 is the orientation matrix of adjacent subgrains, [Q1] -1 q is the inverse of the orientation matrix of the current subgrain. 12 q 13 q 21 q 23 q 31 q 32 The orientation difference matrix Q of each of the two adjacent subgrains 12 Element.
[0255] 6.2) Construct a recrystallization grain growth model.
[0256] Recrystallized grain growth is achieved through grain boundary growth. The conditions for recrystallized grain growth are as follows:
[0257] νΔt≥L cell (7)
[0258] In the formula, L cell It is the length of the cell. Δt is the increment per unit time.
[0259] The grain boundary growth rate ν is determined by both the grain boundary mobility M and the driving force P, as shown below:
[0260] ν=MP (8)
[0261] The grain boundary mobility M is shown below:
[0262]
[0263] In the formula, δ is the grain boundary thickness, and D... ob It is the grain boundary diffusion coefficient at absolute zero, K is the Boltzmann constant, b is the Borgs vector, and Q is the absolute zero temperature. b It is the diffusion activation energy. R is the ideal gas parameter, and T is the deformation temperature.
[0264] Since the presence of second-phase particles significantly hinders the growth of recrystallized grains, the driving force consists not only of the driving force P1 caused by surface energy and the resistance P2 caused by volume energy, but also of the Zener resistance P3 caused by the second-phase particles. The driving force P is shown below:
[0265] P = P1 + P2 + P3 (10)
[0266] The driving force P1 caused by surface energy is shown below:
[0267]
[0268] In the formula, ρ m ρ dThese are the dislocation densities of the matrix grains and recrystallized grains, respectively, and μ is the shear modulus of the material.
[0269] The drag force P2 caused by volume energy is shown below:
[0270]
[0271] In the formula, r d It is the radius of the dynamically recrystallized grain.
[0272] The high-angle grain boundary energy γ is shown below:
[0273]
[0274] In the formula, υ1 is Poisson's ratio. θ m It is the orientation difference angle of the large-angle grain boundary, which is set to 15°.
[0275] The Zener resistance P3 caused by the second-phase particles is shown below:
[0276]
[0277] In the formula, r s f s These are the radius and percentage of the second-phase particles, respectively.
[0278] Example 20:
[0279] A method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata, the main technical contents of which are described in any one of Examples 11 to 19, further comprising the following steps for establishing the continuous recrystallization model:
[0280] 7.1) Initialize the cellular automaton model and define the unit time increment as Δt, with the current time t = 1.
[0281] 7.2) Based on the correspondence between the mesh positions in the mesoscopic finite element model and the cell positions in the cellular automaton model, the cells in the cellular automaton model are numbered, and the deformation temperature, orientation matrix, and dislocation density in the mesoscopic finite element model at the current time t are assigned to the cells.
[0282] 7.3) Scan the cell space and define the color display values of grain boundary cells, recrystallization cells, second phase particle cells, and intragranular cells as 0, 0.5, 1, and 0.75, respectively.
[0283] The recrystallization cell is cell numbered 0.5.
[0284] If the orientation difference angle between two adjacent subgrains is greater than the orientation difference angle θ of a large-angle grain boundary m If so, the current cell number is 0.5.
[0285] The second phase particle cell is cell numbered 0.
[0286] The grain boundary cell is defined as follows: apart from recrystallization cells and second-phase particle cells, if the orientation difference angle between the current cell and any adjacent cell is greater than 15 degrees, then the current cell becomes a grain boundary cell.
[0287] The intragranular cells are the cells remaining excluding grain boundary cells, recrystallization cells, and second-phase particle cells.
[0288] 7.4) Calculate the orientation difference angle of each cell except for the second phase particle cells and grain boundary cells, and determine whether the orientation difference angle of each cell is greater than 15 degrees. If so, the cell nucleation is successful.
[0289] For cells that have successfully formed nuclei, change the current state of the cell and randomly assign a new orientation different from that of the adjacent cells. Increase the recrystallization count by 1, reduce the dislocation density to the initial value, and update the cell number to 0.5.
[0290] 7.5) Determine whether each cell other than the second-phase grain cell has met the grain growth conditions. If so, the current cell state changes and the dislocation density, recrystallization size, orientation and color display value of the current cell are consistent with the target cell.
[0291] The target cell is the neighboring cell of the current cell, that is, the cell in a ring around the current cell. The target cell is calculated sequentially with each cell in the ring around the current cell. When the calculation result satisfies the grain growth condition, the state of the target cell is changed to the state of the cell that was calculated with it.
[0292] 7.6) Determine if t has reached the preset total time step T. If yes, output the recrystallization percentage, recrystallized grain size, and microstructure image. If no, return to step 7.2).
[0293] Example 21:
[0294] See Figures 1 to 2 A method for establishing a continuous dynamic recrystallization model that couples macro-micro finite element models, crystal plasticity, and cellular automata includes the following steps:
[0295] 1) Initial microstructure imaging: Scanning electron microscope (SEM) images and electron backscatter diffraction (EBSD) images of the sample before deformation are obtained by scanning electron microscope. The size of the SEM images and EBSD images must be consistent.
[0296] 2) Establishment of the macroscopic finite element model: A macroscopic finite element model is established in ABAQUS software. This macroscopic finite element model includes the establishment of the hot-compressive geometry model, assignment of material parameters, setting of boundary conditions, and mesh generation;
[0297] 3) Detailed observation of the establishment of the finite element model: The RVE finite element model is established in ABAQUS software.
[0298] 4) Extraction of Euler angles and shear strain rate;
[0299] 5) Calculation of orientation matrix and dislocation density;
[0300] 6) The establishment of the cellular automata model: In order to simulate the evolution of microstructure during hot deformation, the nucleation and growth rules of recrystallized grains need to be defined.
[0301] 7) Establish a continuous recrystallization model through the above steps, and finally determine the algorithm flow of the model;
[0302] The initial microscopic tissue imaging specifically includes the following steps:
[0303] SEM and EBSD images of the sample before deformation were acquired using scanning electron microscopy, ensuring that the dimensions of the SEM and EBSD images were consistent. The dimensions of the EBSD images, the dimensions of small regions within the EBSD images, and the dislocation density and Euler angles of each small region were extracted using OIM software. The pixel locations of the second-phase particle centers in the SEM images were identified using the PIL toolkit in Python, and the dimensions of the second-phase particles in the SEM images were extracted using Image-Pro Plus software.
[0304] The establishment of the macroscopic finite element model, performed in ABAQUS software, specifically includes the following steps:
[0305] A macroscopic finite element model was established in ABAQUS software. This macroscopic finite element model included the establishment of a thermocompressible geometric model, the assignment of material parameters, the setting of boundary conditions, and mesh generation. First, the corresponding geometric models were established based on the dimensions of the actual workpiece and mold. Second, stress-strain curves, elastic parameters, and thermophysical parameters were assigned to the workpiece. Then, boundary conditions were set according to the actual load conditions. Finally, a hexahedral mesh was used to mesh the workpiece, with the mesh size consistent with the size of the small regions in the EBSD image.
[0306] The establishment of the micro-finite element model, which is an RVE finite element model built in ABAQUS software, specifically includes the following steps:
[0307] 3.1) Establish a geometric model of the representative volume element (RVE) containing the second-phase particles. This RVE model is obtained by merging the matrix geometry model and the second-phase particle geometry model. The matrix geometry model is established using the length, width, and micro-region size distribution of the EBSD image as its length, width, and height. The geometry model of the second-phase particles is established based on the extracted second-phase particle size, located at the center of the extracted second-phase particles.
[0308] 3.2) Set the total time and the size of the time increment step.
[0309] 3.3) Mesh the RVE model, with the mesh size matching the size of the small regions in the EBSD diagram.
[0310] 3.4) Sets of matrix and second-phase particles are established separately to assign material parameters to the RVE model. These material parameters include elastic parameters, plastic parameters, thermophysical parameters, and Euler angles extracted from the EBSD image. To map crystal orientations one-to-one to the RVE model, a set is established for each mesh in the model. The set is determined to be either a matrix set or a second-phase particle set based on the geometric positions of the matrix and second-phase particles. The matrix set number is consistent with the mesh number, while the second-phase particle set number is set to 0.
[0311] 3.5) The calculated displacements from the macroscopic numerical simulation results are used as boundary conditions for the mesoscopic finite element model via the SUBMODEL module in ABAQUS. The key to setting these boundary conditions is ensuring that the positions of the mesoscopic finite element model and the macroscopic finite element model are consistent.
[0312] The extraction of the Euler angles and shear strain rate specifically includes the following steps:
[0313] To obtain the Euler angles of each mesh in the mesoscale finite element model, DAMASK was used as the UMAT implementation of ABAQUS to realize the crystal plasticity model as the material constitutive model in the mesoscale finite element model. Based on the mesoscale numerical simulation results, the Euler angles and shear strain rates of each mesh at each time increment step were extracted.
[0314] The calculation of the orientation matrix and dislocation density specifically includes the following steps:
[0315] 5.1) By utilizing the relationship between Euler angles and the orientation matrix, the extracted Euler angles are converted into an orientation matrix, the expression of which is as follows:
[0316]
[0317] 5.2) Based on the modified Kocks and Mecking model and the extracted shear strain rate, the dislocation density for each mesh is calculated. The calculation formula is as follows:
[0318]
[0319] In the formula, ρ is the dislocation density rate of the slip system a. a It is the dislocation density of the slip system a. It is the shear strain rate of slip system a. It relates to the work hardening coefficient. These are coefficients related to dynamic response. Among them, The calculation formula is as follows:
[0320]
[0321] In the formula, n1 is the material parameter, R is the ideal gas parameter, and Q is the ideal gas parameter. act It is the deformation activation energy, and T is the deformation temperature.
[0322] 5.3) The dislocation density of each grid is obtained by superimposing the dislocation density of each slip system.
[0323]
[0324] In the formula, N s It represents the number of slip systems.
[0325] The establishment of the cellular automata model, in order to simulate the evolution of microstructure during hot deformation, requires the definition of the nucleation and growth rules of recrystallized grains, specifically including the following steps:
[0326] 6.1) Recrystallization Grain Nucleation Model
[0327] For continuous dynamic recrystallization, the large-angle grain boundaries of new grains mainly arise from the gradual increase of the orientation difference angle of the subgrains. Therefore, the nucleation rule can be determined by the orientation difference angle of the subgrains. When the orientation difference angle between adjacent subgrains is greater than 15 degrees, the subgrain becomes a recrystallized grain. The orientation difference angle θ can be calculated using the orientation matrix obtained from formula (1). First, calculate the orientation difference matrix Q between two adjacent subgrains. 12 The formula is as follows:
[0328]
[0329] In the formula, Q2 is the orientation matrix of adjacent subgrains, [Q1] -1 It is the inverse of the orientation matrix of the current subcrystal.
[0330] According to formula (5), calculate the orientation difference angle θ:
[0331] θ = arccos(0.5(q) 11 +q 22 +q 33 (6)
[0332] The calculation of this orientation difference serves not only as a condition for recrystallization grain nucleation but also as a basis for defining large-angle grain boundary cells.
[0333] 6.2) Recrystallization Grain Growth Model
[0334] Recrystallized grain growth is achieved through grain boundary growth. The grain boundary growth rate ν is determined by both the grain boundary mobility M and the driving force P, and its expression is as follows:
[0335] ν=MP (7)
[0336] The formula for calculating M is as follows:
[0337]
[0338] In the formula, δ is the grain boundary thickness, and D... ob It is the grain boundary diffusion coefficient at absolute zero, K is the Boltzmann constant, b is the Borgs vector, and Q is the absolute zero temperature. b It is the diffusion activation energy.
[0339] Since the presence of second-phase particles significantly hinders the growth of recrystallized grains, the driving force consists not only of the driving force P1 caused by surface energy and the resistance P2 caused by volume energy, but also of the Zener resistance P3 caused by the second-phase particles. Therefore, the expression for P is as follows:
[0340] P = P1 + P2 + P3 (9)
[0341] The formula for calculating P1 is as follows:
[0342]
[0343] In the formula, ρ m and ρ d These are the dislocation densities of the matrix grains and recrystallized grains, respectively, and μ is the shear modulus of the material.
[0344] The formula for calculating P2 is as follows:
[0345]
[0346] In the formula, r d γ is the radius of the dynamically recrystallized grain, and γ is the high-angle grain boundary energy.
[0347] The formula for calculating γ is as follows:
[0348]
[0349] In the formula, υ is Poisson's ratio. θ m It is the orientation difference angle of the large-angle grain boundary, which is set to 15°.
[0350] The formula for calculating P3 is as follows:
[0351]
[0352] In the formula, r s and f s These are the radius and percentage of the second-phase particles, respectively.
[0353] Substituting formulas (8)-(13) into formula (7) yields the recrystallization grain growth rate. Under a unit time increment, grain growth is successful when the grain boundary growth distance of the recrystallized grain is greater than the cell length. This growth condition is as follows:
[0354] νΔt≥L cell (14)
[0355] In the formula, L cell It is the length of the cell.
[0356] The continuous recrystallization model was established, and the algorithm flow of the model was finally determined. The specific flow is as follows:
[0357] 7.1) Initialize the simulation program and input parameters.
[0358] 7.2) Define the time increment Δt and calculate the current time t.
[0359] 7.3) Based on the correspondence between the mesh position in the meso-finite element model and the cell position in the cellular automaton model, the cells are numbered according to the set number corresponding to the mesh, and the deformation temperature, calculated orientation matrix, and dislocation density in the mesh calculation results of the meso-finite element model at the current moment are assigned to the cells.
[0360] 7.4) Scan the cell space and define grain boundary cells, recrystallization cells, second-phase particle cells, and intragranular cells, with corresponding color display values of 0, 0.5, 1, and 0.75, respectively. The method for determining a second-phase particle cell is that if the current cell number is 0, then that cell is a second-phase particle cell. The method for determining a recrystallization cell is that if the current cell number is 0.5, then that cell is a recrystallization cell. The method for determining a grain boundary cell is that, except for second-phase particle cells and recrystallization cells, if the orientation difference angle between the current cell and any neighboring cell is greater than 15°, then that cell is a grain boundary cell. All cells other than grain boundary cells, second-phase particle cells, and recrystallization cells are intragranular cells.
[0361] 7.5) Calculate the orientation difference angle of each cell except for the second-phase particle cells and grain boundary cells. If the orientation difference angle of the cell is greater than 15°, the cell has successfully nucleated, its cell state is changed, a new orientation different from its neighbors is randomly assigned, the recrystallization number is increased by 1, the dislocation density is reduced to the initial value, and the cell number is updated to 0.5.
[0362] 7.6) Determine whether each cell, except for the second-phase grain cells, meets the grain growth condition. If the condition is met, the state of the cell changes, and the dislocation density, recrystallization size, orientation, and color display value of the current cell become consistent with those of the target cell.
[0363] 7.7) Steps 7.3)-7.6) constitute a loop step, which is repeated until the set total time step T is reached.
[0364] 7.8) Statistical analysis of recrystallization percentage, recrystallized grain size, and output of microstructure images.
[0365] Example 22:
[0366] A method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata is described in Example 21. Further, the method includes the following:
[0367] 1. Determine the experimental subjects
[0368] Material: 2219 aluminum alloy
[0369] Process: Hot compression, temperature 450℃, strain rate 0.52
[0370] 2. Input parameters
[0371] 1) Initial microscopic tissue imaging
[0372] The size of both EBSD and SEM images was set to 1800um × 1800um.
[0373] The step size for capturing EBSD images was set to 9µm.
[0374] 2) Macroscopic finite element model
[0375] Geometry: The workpiece is a cylindrical sample with dimensions of Φ8mm×12mm, and the mold is a cuboid with dimensions of 20mm×20mm×1mm.
[0376] Time: Total time is 0.77s, time increment step is 0.01.
[0377] Material parameters: stress-strain curves as shown Figure 2 As shown, other parameters are listed in Table 1.
[0378] Table 12219 Aluminum Alloy Parameters
[0379]
[0380] Boundary conditions: The mold moves in the height direction of the workpiece, and the mold moves at a speed of 6.23 mm / s.
[0381] Grid: Grid type, grid size.
[0382] 3) Microscopic finite element model and crystal plasticity model
[0383] Geometric parameters: The dimensions of the RVE geometry are 1800um x 1800um x 9um. The coordinates of the center position of the second phase particles are shown in Appendix A. The average radius of the second phase particles is 2.5um.
[0384] Time: Total time is 0.77s, time increment step is 0.01.
[0385] Mesh: The mesh type is a hexahedral mesh, and the mesh size is 9µm.
[0386] Material parameters related to crystal plasticity: Material parameters of the matrix are listed in Tables 2 and 3, and material parameters of the second phase particles are listed in Tables 4 and 5.
[0387] Table 2 Thermophysical parameters of the second-phase particles
[0388]
[0389] Table 3 Grain plasticity parameters of the second phase particles
[0390]
[0391] Table 4 Thermophysical parameters of the matrix
[0392]
[0393] Table 5 Grain plasticity parameters of the matrix
[0394]
[0395] Boundary conditions: Calculated displacements from macroscopic simulation results.
[0396] The parameters of the KM model are listed in Table 6.
[0397] Table 6 Parameters in the KM model
[0398]
[0399] 4) Cellular automata model
[0400] Cell: The cell type is a cube, and the cell size is 9um x 9um.
[0401] Cellular space: The space size is 1800um x 1800um, and this space is divided into square grids.
[0402] Cellular state variables: deformation temperature, dislocation density, orientation matrix
[0403] Cell numbering: matrix number, second phase particle number. The matrix number is consistent with the mesh number in the micro finite element model, and the second phase particle number is set to 0.
[0404] Cell color display values: Grain boundary cells, recrystallization cells, second-phase particle cells, and intragranular cells, with corresponding color display values set to 0, 0.5, 1, and 0.75, respectively.
[0405] Neighbor type: Von Neumann type.
[0406] Boundary conditions: Periodic boundary conditions.
[0407] Time increment: The time increment is set to 0.01s, and the total time is 0.77s.
[0408] Table 7 Material parameters for cellular automata
[0409] parameter numerical values <![CDATA[δD ob (m2s-1)]]> 3.77×10-12 b(m) 2.86×10-10 K(JK-1) 1.38×10-23 <![CDATA[Q b (Jmod-1)]]> 70000 υ 0.33 <![CDATA[ρ d (m-2)]]> 1.0×1010 R(JK⁻¹mol⁻¹) 8.3145 μ(Pa) 5.45×106 <![CDATA[r s (m)]]> 2.56×10-6 <![CDATA[f s (%)]]> 3.88
[0410] Material parameters: The parameters are listed in Table 7.
[0411] 3. Implementation process, the specific steps are as follows:
[0412] 1) Based on the set image size and step size, SEM and EBSD images of 2219 aluminum alloy were captured before the hot compression experiment. The dislocation density and Euler angles of each small region in the EBSD image were extracted. The pixel positions of the second-phase particle centers in the SEM image were identified, and the size of the second-phase particles in the SEM image was extracted.
[0413] 2) Based on the known parameters, establish a finite element model of hot compression of 2219 aluminum alloy in ABAQUS and obtain the calculated displacement in the numerical simulation results.
[0414] 3) Based on the known parameters, establish an RVE finite element model containing second-phase particles in ABAQUS, and use the calculated displacement in the macroscopic simulation results as the boundary conditions of the RVE finite element model.
[0415] 4) Using DAMASK as the UMAT in the mesoscopic finite element model, extract the deformation temperature, Euler angle, and shear strain rate of each mesh at each time increment step in the mesoscopic simulation results.
[0416] 5) According to formula (1), the extracted Euler angles are calculated into an orientation matrix. According to formulas (2)-(4), the extracted shear strain rate is calculated into a dislocation density.
[0417] 6) Initialize the cellular automaton program and input the parameters.
[0418] 7) Define the time increment Δt and calculate the current time t.
[0419] 8) Based on the correspondence between the mesh position in the meso-finite element model and the cell position in the cellular automaton model, the cells are numbered according to the set number corresponding to the mesh, and the deformation temperature, calculated orientation matrix, and dislocation density in the mesh calculation results of the meso-finite element model at the current time t are assigned to the cells.
[0420] 9) Scan the cell space and define grain boundary cells, recrystallization cells, second-phase particle cells, and intragranular cells respectively. Their corresponding color display values are 0, 0.5, 1, and 0.75, respectively. The method for determining second-phase particle cells is that if the current cell number is 0, then the cell is a second-phase particle cell. The method for determining recrystallization cells is that if the current cell number is 0.5, then the cell is a recrystallization cell. The method for determining grain boundary cells is that, except for second-phase particle cells and recrystallization cells, the orientation difference angle between the current cell and any neighboring cell is calculated according to formula (5). If the angle is greater than 15°, then the cell is a grain boundary cell. Except for grain boundary cells, second-phase particle cells, and recrystallization cells, other cells are intragranular cells.
[0421] 10) Calculate the orientation difference angle of each cell except for the second phase particle cells and grain boundary cells according to formulas (5) and (6). If the orientation difference angle of the cell is greater than 15°, the cell nucleation is successful, its cell state is changed, a new orientation different from its neighbors is randomly assigned, the recrystallization number is increased by 1, the dislocation density is reduced to the initial value, and the cell number is updated to 0.5.
[0422] 11) Calculate the recrystallization grain growth rate according to formulas (7)-(13). Substitute the calculated growth rate into formula (14) to determine whether each cell except the second phase grain cell meets the grain growth condition. If the condition is met, the cell state changes, and the dislocation density, recrystallization size, orientation, and color display value of the current cell are consistent with the target cell.
[0423] 12) Steps 7)-11) constitute a loop step, which is repeated until the set total time step T is reached.
[0424] 13) Calculate the recrystallization percentage, recrystallized grain size, and output microstructure images.
Claims
1. A method for establishing a continuous dynamic recrystallization model coupling macro-mesoscopic finite element model, crystal plasticity and cellular automaton, characterized in that, Includes the following steps: 1) Obtain SEM and EBSD images of the workpiece material before deformation, and extract the geometric parameters from the SEM and EBSD images; 2) Establish a macroscopic finite element model; 3) Based on the macroscopic finite element model and the geometric parameters in the SEM and EBSD images, a microscopic finite element model is established; 4) Extract the Euler angles and shear strain rate from the mesoscopic finite element model; 5) Based on Euler angles and shear strain rate, the corresponding orientation matrix and dislocation density are calculated; 6) Based on the orientation matrix and dislocation density, establish a cellular automata model. The steps include: 6.1) Construct a recrystallization grain nucleation model using the orientation difference angle of subgrains; If the orientation difference angle between the current subcrystal and any adjacent subcrystal is greater than x degrees, then the current subcrystal is a recrystallized grain, where x is a positive number; The orientation difference angle between the two adjacent subgrains is shown below: (1) In the formula, The orientation difference angle between two adjacent subcrystals; , , Both are orientation difference matrices of two adjacent subcrystals. The diagonal elements; Among them, the orientation difference matrix of two adjacent subcrystals As shown below: (2) In the formula, The orientation matrix of adjacent subgrains. This is the inverse of the orientation matrix of the current subcrystal; , , , , , Both are orientation difference matrices of two adjacent subcrystals. Element; 6.2) Construct a recrystallization grain growth model; The conditions for the growth of the recrystallized grains are as follows: (3) In the formula, It is the length of the cell; Increment per unit time; Among them, grain boundary growth rate As shown below: (4) Among them, grain boundary mobility As shown below: (5) In the formula, It is the grain boundary thickness. It is the grain boundary diffusion coefficient at absolute zero, and K is the Boltzmann constant. It is a Boges vector. It is the diffusion activation energy; R is the ideal gas parameter, and T is the deformation temperature; driving force As shown below: (6) Among them, the driving force caused by surface energy As shown below: (7) In the formula, , These are the dislocation densities of the matrix grains and recrystallized grains, respectively. It is the shear modulus of the material; drag caused by volume energy As shown below: (8) In the formula, It is the radius of the dynamically recrystallized grain; Among them, high-angle grain boundary energy As shown below: (9) In the formula, It is Poisson's ratio; It is the orientation difference angle of a large-angle grain boundary; Zener drag caused by second-phase particles As shown below: (10) In the formula, , These are the radius and percentage of the second-phase particles, respectively. 7) Return to step 4) to perform the calculation of the next incremental step until the prediction of the dynamic recrystallization evolution coupling response is completed and the continuous recrystallization model is established.
2. The method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata as described in claim 1, characterized in that, The geometric parameters in the SEM and EBSD images include the size of the EBSD image, the size of the micro-regions in the EBSD image, the dislocation density and Euler angles of each micro-region in the EBSD image, the pixel position of the center of the second-phase particles in the SEM image, and the size of the second-phase particles in the SEM image.
3. The method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata as described in claim 1, characterized in that, The steps for establishing the macroscopic finite element model include: 2.1) Establish a thermal compression geometric model based on the actual dimensions of the workpiece; 2.2) Assign stress-strain curves, elastic parameters, and thermophysical parameters to the hot-compression geometric model; 2.3) Set load boundary conditions based on the actual load and mold conditions; 2.4) The thermal compression geometric model is meshed using a hexahedral mesh.
4. The method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata as described in claim 1, characterized in that, The steps for establishing a micro-finite element model based on the macro-finite element model and geometric parameters in SEM and EBSD images include: 3.1) By merging the matrix geometric model and the second-phase particle geometric model, a representative volume element geometric model containing the second-phase particles is established; The matrix geometric model is established using the length, width, and micro-region size distribution of the EBSD image as its length, width, and height. The geometric model of the second phase particles is established based on the size of the second phase particles in the SEM image, at the position of the center of the second phase particles; 3.2) Mesh the geometric model of the representative volume element containing second-phase particles; 3.3) Assign material parameters to the geometric model of the representative volume element containing second-phase particles; 3.4) Set the calculated displacement in the numerical simulation results of the macroscopic finite element model as the load boundary condition of the microscopic finite element model.
5. The method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata as described in claim 4, characterized in that, The material parameters include elastic parameters, plastic parameters, thermophysical parameters, and Euler angles.
6. The method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata as described in claim 4, characterized in that, The steps for assigning material parameters to the geometric model of the representative volume element containing second-phase particles are as follows: 3.3.1) Number each mesh in the representative volume element geometric model containing second-phase particles; 3.3.2) Based on the geometric positions of the matrix and the second-phase particles, determine whether each grid in the geometric model of the representative volume element containing the second-phase particles corresponds to the matrix. If yes, the grid number remains unchanged; otherwise, the grid number is set to 0. 3.3.3) Assign the material parameters of the second phase particles to the mesh numbered 0, and assign the material parameters of the matrix to the meshes not numbered 0.
7. The method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata as described in claim 1, characterized in that, The orientation matrix is shown below: (11) In the formula, For orientation matrix; , , Both represent Euler angles.
8. The method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata according to claim 1, characterized in that, The dislocation density is shown below: (12) In the formula, This represents the dislocation density of each grid cell; Indicates the slip coefficient ordinal number; It is the number of slip systems; Indicates the slip system Dislocation density; Among them, slip system dislocation density The result is obtained by formula (3): (13) In the formula, It is a slip system dislocation density rate, It is a slip system shear strain rate, It is a coefficient related to work hardening; Among them, the coefficients related to dynamic response As shown below: (14) In the formula, and All represent material parameters, and R is the ideal gas parameter. It is the deformation activation energy, and T is the deformation temperature.
9. The method for establishing a continuous dynamic recrystallization model coupled with a macro-micro finite element model, crystal plasticity, and cellular automata according to claim 1, characterized in that, The steps for establishing the continuous recrystallization model include: 7.1) Initialize the cellular automaton model and define the unit time increment as... The current time is t=1; 7.2) Based on the correspondence between the mesh positions in the mesoscopic finite element model and the cell positions in the cellular automaton model, the cells in the cellular automaton model are numbered, and the deformation temperature, orientation matrix, and dislocation density in the mesoscopic finite element model at the current time t are assigned to the cells. 7.3) Scan the cell space and define the color display values of grain boundary cells, recrystallization cells, second-phase particle cells, and intragranular cells as 0, 0.5, 1, and 0.75, respectively; The recrystallized cell is cell numbered 0.5; If the orientation difference angle between two adjacent subgrains is greater than the orientation difference angle of a large-angle grain boundary If so, the current cell number is 0.5; The second phase particle cell is the cell numbered 0; The grain boundary cell is defined as follows: apart from recrystallization cells and second-phase particle cells, if the orientation difference angle between the current cell and any adjacent cell is greater than x degrees, then the current cell becomes a grain boundary cell, where x is a positive number. The intragranular cells are the cells remaining excluding grain boundary cells, recrystallization cells, and second-phase particle cells; 7.4) Calculate the orientation difference angle of each cell except for the second phase particle cells and grain boundary cells, and determine whether the orientation difference angle of each cell is greater than x degrees. If so, the cell nucleation is successful. For cells that have successfully formed nuclei, change the current state of the cell and randomly assign a new orientation different from that of the adjacent cells. Increase the recrystallization count by 1, reduce the dislocation density to the initial value, and update the cell number to 0.
5. 7.5) Determine whether each cell other than the second phase grain cell meets the grain growth conditions. If so, the current cell state changes and the dislocation density, recrystallization size, orientation and color display value of the current cell are consistent with the target cell. The target cell is the neighboring cell of the current cell; 7.6) Determine whether t has reached the preset total time step T. If yes, output the recrystallization percentage, recrystallized grain size, and microstructure image; otherwise, return to step 7.2.
Citation Information
Patent Citations
Method for predicting coupling responses of isothermal forming and dynamic recrystallization evolution of titanium alloys
CN106202675A
Method for damage evolution simulation of bituminous mixture based on cellular automation model
CN107145670A