A type of BiO(IO3) 1-x (VO3) x Photocatalysts, their preparation methods and applications
By introducing VO₃⁻ ions into the BiOIO₃ lattice, altering its nanostructure, and introducing oxygen vacancies, the problems of insufficient response to ultraviolet light and low separation efficiency of photogenerated electron-hole pairs in the BiOIO₃ photocatalyst were solved, achieving efficient photocatalytic degradation of antibiotics.
Patent Information
- Application Number
- CN202410265406.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-08
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-03-08
AI Technical Summary
Existing BiOIO₃ photocatalysts are inefficient in photocatalytic degradation of antibiotics due to their wide bandgap characteristics, which only respond to ultraviolet light and the high surface recombination rate of photogenerated electron-hole pairs.
By introducing VO₃⁻ ions into the BiOIO₃ lattice, a BiO(IO₃)₁₋ₓ(VO₃)ₓ photocatalyst is formed, changing its microstructure to a nanoribbon morphology. Furthermore, I⁻/I⁵⁺ redox pairs and oxygen vacancies are introduced into the lattice to promote bulk separation of photogenerated carriers.
The visible light absorption capacity and photogenerated electron-hole pair separation efficiency of the BiO(IO₃)₁₋ₓ(VO₃)ₓ photocatalyst were improved, enhancing the photocatalytic degradation effect on antibiotics, especially under ultraviolet light and simulated sunlight.
Smart Images

Figure HDA0004732182710000011 
Figure HDA0004732182710000012 
Figure HDA0004732182710000013
Abstract
Description
Technical Field
[0001] This invention belongs to the field of functional materials, specifically relating to a BiO(IO3) compound. 1-x (VO3) x Photocatalysts, their preparation methods, and applications. Background Technology
[0002] Traditional methods for removing antibiotics from the environment and wastewater, such as physicochemical adsorption, electrochemical regeneration, biodegradation, and membrane filtration, are complex to operate, energy-intensive, and may cause secondary pollution, which is inconsistent with the concept of green and environmentally friendly development. Furthermore, these methods show relatively poor performance in removing low concentrations of antibiotics. Photocatalytic oxidation technology, due to its low energy consumption, mild reaction conditions, non-toxicity, high efficiency, low cost, and environmental friendliness, has attracted widespread attention in the field of environmental remediation.
[0003] The key to the practical application of photocatalytic oxidation technology lies in the selection of semiconductor photocatalytic materials. In recent years, Bi-based semiconductor materials, represented by BiVO4, Bi2WO6, Bi2O3, BiOX (X = Cl, Br, I), Bi2O2CO3, and BiOIO3, have attracted widespread attention in the field of photocatalysis. Among these materials, BiOIO3 is a novel Bi-based semiconductor photocatalyst, characterized by its low cost, non-toxicity, unique physicochemical properties, and environmental friendliness. Furthermore, BiOIO3 is composed of [Bi2O2]... 2+ Layers and IO3 - Composed of alternating layers, its unique layered structure induces a built-in polarized electric field within the crystal, which is beneficial for the bulk separation of photogenerated electron-hole pairs. Even so, the practical application of BiOIO3 is still limited by the following reasons: (1) BiOIO3 is a typical wide bandgap semiconductor material with a bandgap energy of about 3.2 eV, and only responds to ultraviolet light, which accounts for 4%-5% of the solar spectrum; (2) The surface recombination rate of photogenerated electron-hole pairs is high, and the utilization rate of charge carriers is low. Summary of the Invention
[0004] The purpose of this invention is to provide a BiO(IO3) solution. 1-x (VO3) x Photocatalysts, their preparation methods, and applications; BiO(IO3) prepared. 1-x (VO3) x The photocatalyst exhibits enhanced visible light absorption and its photogenerated electron-hole pairs have high separation efficiency.
[0005] This invention is achieved through the following technical solution:
[0006] A type of BiO(IO3) 1-x (VO3) xA photocatalyst, wherein the chemical formula of the photocatalyst is BiO(IO3). 1-x (VO3) x Where x is 0.02-0.06, the photocatalyst exhibits a nanoribbon morphology.
[0007] Preferably, x is 0.04, and the photocatalyst exhibits a nanoribbon morphology with serrated edges.
[0008] The BiO(IO3) mentioned above 1-x (VO3) x The preparation method of the photocatalyst includes the following steps:
[0009] Step 1: Disperse Bi(NO3)3·5H2O powder into HNO3 solution and stir to obtain suspension A;
[0010] Step 2: Under stirring conditions, add KIO3 powder to suspension A and stir to obtain suspension B;
[0011] Step 3: Under stirring conditions, add NH4VO3 powder to suspension B and stir to obtain reaction precursor solution C;
[0012] Step 4: Perform a hydrothermal reaction on the precursor solution C; after the reaction is complete, wash and dry the resulting precipitate to obtain BiO(IO3). 1-x (VO3) x Photocatalyst.
[0013] Preferably, in the reaction precursor solution C obtained in step 3, the molar ratio of Bi(NO3)3·5H2O to the sum of the molar amounts of KIO3 and NH4VO3 is 1:(1.02-1.06).
[0014] Preferably, in the reaction precursor solution C obtained in step 3, the concentrations of Bi(NO3)3·5H2O, HNO3, KIO3, and NH4VO3 are 0.020-0.067 mol·L⁻¹. -1 0.015-0.045 mol·L -1 0.020-0.067 mol·L -1 and 0.0005-0.004 mol·L -1 .
[0015] Preferably, in step 4, the hydrothermal reaction temperature is 150-210℃ and the reaction time is 18-32h.
[0016] Preferably, the hydrothermal reactor used for the hydrothermal reaction has a filling ratio of 60%-80%.
[0017] Preferably, in step 4, the drying temperature is 50-80℃.
[0018] The BiO(IO3) mentioned above 1-x (VO3) x Application of photocatalysts in the photocatalytic degradation of organic pollutants.
[0019] Preferably, the organic pollutant is an antibiotic.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The BiO(IO3) described in this invention 1-x (VO3) x Photocatalyst, introducing VO3 into the BiOIO3 lattice - After the addition of ionic groups, the microstructure of the catalyst changes from an irregular nanosheet morphology to a nanoribbon morphology, and I- exists in its crystal lattice. - / I 5+ Redox pairs and oxygen vacancies; VO3 - The introduction of ionic groups promotes the development of BiO(IO3). 1-x (VO3) x Growing along the c-axis, the resulting macroscopic polarization electric field can promote bulk phase separation of photogenerated carriers; VO3 - The introduction of ionic groups makes BiO(IO3) more... 1-x (VO3) x An increase in the oxygen vacancy concentration in the photocatalyst lattice, with oxygen vacancies serving as charge trapping centers and active sites, can provide directional transfer channels for photogenerated electrons, thereby improving the surface separation efficiency of photogenerated electron-hole pairs. Furthermore, due to I... - / I 5+ The synergistic effect of redox pairs and oxygen vacancies in BiO(IO3) 1-x (VO3) x The visible light absorption of the photocatalyst is significantly enhanced, improving its utilization rate of solar energy. Therefore, the BiO(IO3) prepared in this invention... 1-x (VO3) x The photocatalyst exhibits enhanced photocatalytic activity, and under ultraviolet light and simulated sunlight irradiation, it can mineralize antibiotics such as tetracycline hydrochloride, ciprofloxacin, ofloxacin, norfloxacin, oxytetracycline, and metronidazole into H2O and CO2.
[0022] Furthermore, when x is 0.04, the photocatalyst exhibits a nanoribbon morphology with serrated edges, and the formation of serrated edges further enhances the properties of BiO(IO3). 1-x (VO3) x The oxygen vacancy concentration in the photocatalyst lattice increases. Attached Figure Description
[0023] Figure 1 The BiO(IO3) prepared in this invention 1-x (VO3) x XRD patterns of photocatalyst powder;
[0024] Figure 2 The BiO(IO3) prepared in this invention 1-x (VO3) x Amplified diffraction peaks in the XRD pattern of photocatalyst powder within the range of 26.5°–28.5°;
[0025] Figure 3 The BiO(IO3) prepared in this invention 1-x (VO3) x FT-IR spectra of photocatalyst powders;
[0026] Figure 4 The BiO(IO3) prepared in this invention 1-x (VO3) x The FT-IR spectrum of photocatalyst powder at 700 cm⁻¹ -1 -800cm -1 Amplified characteristic absorption peaks within the range;
[0027] Figure 5 The BiO(IO3) prepared in this invention 1-x (VO3) x Raman spectra of photocatalyst powders;
[0028] Figure 6 The BiO(IO3) prepared in this invention 1-x (VO3) x SEM image of photocatalyst powder;
[0029] Figure 7 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 Elemental mapping diagram of photocatalyst powder;
[0030] Figure 8 The BiO(IO3) prepared in this invention 1-x (VO3) x EPR spectrum of photocatalyst powder;
[0031] Figure 9 The BiO(IO3) prepared in this invention 1-x (VO3) x High-resolution XPS Bi4f spectra of photocatalyst powder;
[0032] Figure 10 The BiO(IO3) prepared in this invention1-x (VO3) x High-resolution XPS O 1s spectrum of photocatalyst powder;
[0033] Figure 11 The BiO(IO3) prepared in this invention 1-x (VO3) x High-resolution XPS I 3d spectra of photocatalyst powder;
[0034] Figure 12 The BiO(IO3) prepared in this invention 1-x (VO3) x N2 adsorption-desorption isotherms of photocatalyst powder;
[0035] Figure 13 The BiO(IO3) prepared in this invention 1-x (VO3) x Pore size distribution curve of photocatalyst powder;
[0036] Figure 14 The BiO(IO3) prepared in this invention 1-x (VO3) x The ultraviolet-visible diffuse reflectance spectrum of photocatalyst powder;
[0037] Figure 15 The BiO(IO3) prepared in this invention 1-x (VO3) x Kubelka-Munk conversion curves of UV-Vis diffuse reflectance spectra of photocatalyst powders;
[0038] Figure 16 The BiO(IO3) prepared in this invention 1-x (VO3) x Degradation curve of photocatalyst powder on tetracycline hydrochloride under ultraviolet light irradiation;
[0039] Figure 17 The BiO(IO3) prepared in this invention 1-x (VO3) x Kinetic curves of photocatalytic degradation of tetracycline hydrochloride by photocatalyst powder under ultraviolet light irradiation;
[0040] Figure 18 The BiO(IO3) prepared in this invention 1-x (VO3) x Degradation curves of photocatalyst powder on tetracycline hydrochloride under simulated sunlight irradiation;
[0041] Figure 19 The BiO(IO3) prepared in this invention 1-x (VO3) xKinetic curves of photocatalyst powder photocatalytic degradation of tetracycline hydrochloride under simulated sunlight irradiation;
[0042] Figure 20 The BiO(IO3) prepared in this invention 1-x (VO3) x Degradation curves of ciprofloxacin by photocatalyst powder under simulated sunlight irradiation;
[0043] Figure 21 The BiO(IO3) prepared in this invention 1-x (VO3) x Kinetic curves of photocatalyst powder photocatalytic degradation of ciprofloxacin under simulated sunlight irradiation;
[0044] Figure 22 The BiO(IO3) prepared in this invention 1-x (VO3) x Total organic carbon (TOC) removal rate of photocatalyst powder during the degradation of tetracycline hydrochloride and ciprofloxacin under simulated sunlight irradiation;
[0045] Figure 23 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 Degradation curves of photocatalyst powder on tetracycline, ofloxacin, norfloxacin and metronidazole under simulated sunlight irradiation;
[0046] Figure 24 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 Kinetic curves of photocatalyst powder photocatalytic degradation of tetracycline, ofloxacin, norfloxacin and metronidazole under simulated sunlight irradiation;
[0047] Figure 25 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 TOC removal rate of photocatalyst powder during simulated sunlight irradiation to degrade tetracycline, ofloxacin, norfloxacin and metronidazole;
[0048] Figure 26 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 Results of a cyclic experiment on the photocatalytic degradation of tetracycline hydrochloride by photocatalyst powder under simulated sunlight irradiation;
[0049] Figure 27 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 XRD patterns of photocatalyst powder before and after cyclic reaction;
[0050] Figure 28 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 UV-Vis diffuse reflectance spectra of photocatalyst powder before and after cyclic reaction;
[0051] Figure 29 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 EPR spectra of photocatalyst powder before and after cyclic reaction;
[0052] Figure 30 The BiO(IO3) prepared in this invention 1-x (VO3) x Transient photocurrent response curve of photocatalyst powder under simulated sunlight irradiation;
[0053] Figure 31 The BiO(IO3) prepared in this invention 1-x (VO3) x Electrochemical impedance spectroscopy of photocatalyst powder under simulated sunlight irradiation;
[0054] Figure 32 The BiO(IO3) prepared in this invention 1-x (VO3) x Photoluminescence spectrum of photocatalyst powder in the range of 330 nm to 600 nm;
[0055] Figure 33 The BiO(IO3) prepared in this invention 1-x (VO3) x Photoluminescence spectrum of photocatalyst powder in the range of 580 nm-700 nm;
[0056] Figure 34 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 Results of active species capture experiment of photocatalyst powder in photocatalytic degradation of tetracycline hydrochloride under simulated sunlight irradiation;
[0057] Figure 35 The Mott-Schottky curves of the BiOIO3 photocatalyst powder prepared in Comparative Example 1 are shown.
[0058] Figure 36 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 Mott-Schottky curves of photocatalyst powders;
[0059] Figure 37The BiO(IO3) prepared in this invention 1-x (VO3) x Photocatalytic mechanism of photocatalyst powder under simulated sunlight irradiation;
[0060] Figure 38 The time-resolved fluorescence spectrum of the BiOIO3 photocatalyst powder prepared in Comparative Example 1 is shown.
[0061] Figure 39 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 Time-resolved fluorescence spectra of photocatalyst powders;
[0062] Figure 40 The BiO(IO3) prepared in this invention 1-x (VO3) x EPR spectrum of superoxide radicals in photocatalyst powder under simulated sunlight irradiation;
[0063] Figure 41 The BiO(IO3) prepared in this invention 1-x (VO3) x EPR spectrum of hydroxyl radicals in photocatalyst powder under simulated sunlight irradiation. Detailed Implementation
[0064] To further understand the present invention, the present invention will be described below with reference to embodiments. These descriptions are only for further explaining the features and advantages of the present invention and are not intended to limit the claims of the present invention.
[0065] The BiO(IO3) described in this invention 1-x (VO3) x A photocatalyst, wherein the chemical formula of the photocatalyst is BiO(IO3). 1-x (VO3) x Where x is 0.02-0.06; the photocatalyst exhibits a nanoribbon morphology, and I exists in its lattice. - / I 5+ Redox pairs and oxygen vacancy defects. When x is 0.04, the catalyst morphology is a nanoribbon morphology with serrated edges.
[0066] The BiO(IO3) 1-x (VO3) x The preparation method of the photocatalyst includes the following steps:
[0067] Step 1: Disperse Bi(NO3)3·5H2O powder into HNO3 solution and stir to obtain a uniform suspension A;
[0068] Step 2: Under stirring conditions, add KIO3 powder to the above suspension A, and continue stirring for a certain period of time to obtain a uniform suspension B;
[0069] Step 3: Under stirring conditions, add NH4VO3 powder to the above suspension B, and continue stirring for a certain period of time to obtain a uniformly mixed reaction precursor solution C;
[0070] Step 4: Transfer the above-mentioned precursor solution C to a hydrothermal reactor for hydrothermal reaction; after the reaction is completed, wash and dry the resulting precipitate to obtain BiO(IO3). 1-x (VO3) x Photocatalyst.
[0071] The ratio of the molar amount of Bi(NO3)3·5H2O to the sum of the molar amounts of KIO3 and NH4VO3 in the reaction precursor solution obtained in step 3 is: m(Bi(NO3)3·5H2O):m(KIO3+NH4VO3)=1:(1.02-1.06).
[0072] In the reaction precursor solution obtained in step 3, the concentrations of Bi(NO3)3·5H2O, HNO3, KIO3, and NH4VO3 were 0.020-0.067 mol·L⁻¹, respectively. -1 0.015-0.045 mol·L -1 0.020-0.067 mol·L -1 and 0.0005-0.004 mol·L -1 .
[0073] In step 4, the hydrothermal reaction temperature is 150-210℃, the reaction time is 18-32h, and the filling ratio of the hydrothermal reactor is 60%-80%.
[0074] In step 4, the drying temperature is 50-80℃.
[0075] The BiO(IO3) obtained by the preparation method described above 1-x (VO3) x The photocatalyst exhibits a nanoribbon morphology with serrated edges, and its lattice contains Ig. - / I 5+ Redox pairs and oxygen vacancy defects.
[0076] The BiO(IO3) obtained by the preparation method described above 1-x (VO3) x The photocatalyst exhibits strong visible light absorption and high photogenerated carrier separation efficiency. Under ultraviolet light and simulated sunlight irradiation, it can decompose antibiotics into H2O and CO2. The antibiotics are tetracycline hydrochloride, ciprofloxacin, ofloxacin, norfloxacin, oxytetracycline, and metronidazole.
[0077] Comparative Example 1
[0078] Step 1: Disperse 2 mmol (0.970 g) of Bi(NO3)3·5H2O powder into 30 mL of 0.03 mol·L⁻¹ solution. -1 After magnetic stirring in the HNO3 solution for 30 minutes, a uniform suspension A was obtained.
[0079] Step 2: While magnetically stirring, add 2 mmol (0.428 g) of KIO3 powder to the above suspension A, stir for 30 min, and obtain a uniform reaction precursor solution B;
[0080] Step 3: Transfer the precursor solution B to a hydrothermal reactor with a filling ratio of 70% and react at 180°C for 24 hours. After the reaction, wash the precipitate three times with deionized water and anhydrous ethanol respectively, and dry it at 70°C for 12 hours to obtain BiOIO3 photocatalyst powder.
[0081] Example 1
[0082] Step 1: Disperse 2 mmol (0.970 g) of Bi(NO3)3·5H2O powder into 30 mL of 0.03 mol·L⁻¹ solution. -1 After magnetic stirring in the HNO3 solution for 30 minutes, a uniform suspension A was obtained.
[0083] Step 2: While magnetically stirring, add 2 mmol (0.428 g) of KIO3 powder to the above suspension A, stir for 30 min to obtain a uniform suspension B;
[0084] Step 3: While magnetically stirring, add 0.04 mmol (0.005 g) of NH4VO3 powder to the above suspension B, and stir for 30 min to obtain a well-mixed reaction precursor solution C;
[0085] Step 4: Transfer the precursor solution C to a hydrothermal reactor with a filling ratio of 70%, and react at 180°C for 24 hours. After the reaction, wash the resulting precipitate three times with deionized water and anhydrous ethanol, and dry it at 80°C for 12 hours to obtain BiO(IO3). 0.98 (VO3) 0.02 Photocatalyst powder.
[0086] Example 2
[0087] Step 1: Disperse 2 mmol (0.970 g) of Bi(NO3)3·5H2O powder into 30 mL of 0.03 mol·L⁻¹ solution. -1After magnetic stirring in the HNO3 solution for 30 minutes, a uniform suspension A was obtained.
[0088] Step 2: While magnetically stirring, add 2 mmol (0.428 g) of KIO3 powder to the above suspension A, stir for 30 min to obtain a uniform suspension B;
[0089] Step 3: While magnetically stirring, add 0.08 mmol (0.009 g) of NH4VO3 powder to the above suspension B, and stir for 30 min to obtain a well-mixed reaction precursor solution C;
[0090] Step 4: Transfer the precursor solution C to a hydrothermal reactor with a filling ratio of 70% and react at 180°C for 24 hours. After the reaction, wash the resulting precipitate three times with deionized water and anhydrous ethanol, and dry it at 70°C for 12 hours to obtain BiO(IO3). 0.96 (VO3) 0.04 Photocatalyst powder.
[0091] Example 3
[0092] Step 1: Disperse 2 mmol (0.970 g) of Bi(NO3)3·5H2O powder into 30 mL of 0.03 mol·L⁻¹ solution. -1 After magnetic stirring in the HNO3 solution for 30 minutes, a uniform suspension A was obtained.
[0093] Step 2: While magnetically stirring, add 2 mmol (0.428 g) of KIO3 powder to the above suspension A, stir for 30 min to obtain a uniform suspension B;
[0094] Step 3: While magnetically stirring, add 0.12 mmol (0.014 g) of NH4VO3 powder to the above suspension B, and stir for 30 min to obtain a well-mixed reaction precursor solution C;
[0095] Step 4: Transfer the precursor solution C to a hydrothermal reactor with a filling ratio of 70% and react at 180°C for 24 hours. After the reaction, wash the resulting precipitate three times with deionized water and anhydrous ethanol, and dry it at 60°C for 12 hours to obtain BiO(IO3). 0.94 (VO3) 0.06 Photocatalyst powder.
[0096] Example 4
[0097] Step 1: Disperse 2 mmol (0.970 g) of Bi(NO3)3·5H2O powder into 100 mL of 0.015 mol·L⁻¹ solution. -1After magnetic stirring in the HNO3 solution for 30 minutes, a uniform suspension A was obtained.
[0098] Step 2: While magnetically stirring, add 2 mmol (0.428 g) of KIO3 powder to the above suspension A, stir for 30 min to obtain a uniform suspension B;
[0099] Step 3: While magnetically stirring, add 0.08 mmol (0.009 g) of NH4VO3 powder to the above suspension B, and stir for 30 min to obtain a well-mixed reaction precursor solution C;
[0100] Step 4: Transfer the precursor solution C to a hydrothermal reactor with a filling ratio of 60%, and react at 150°C for 32 hours. After the reaction, wash the resulting precipitate three times with deionized water and anhydrous ethanol, and dry it at 50°C for 25 hours to obtain BiO(IO3). 0.94 (VO3) 0.06 Photocatalyst powder.
[0101] Example 5
[0102] Step 1: Disperse 2 mmol (0.970 g) of Bi(NO3)3·5H2O powder into 60 mL of a 0.045 mol·L⁻¹ solution. -1 After magnetic stirring in the HNO3 solution for 30 minutes, a uniform suspension A was obtained.
[0103] Step 2: While magnetically stirring, add 2 mmol (0.428 g) of KIO3 powder to the above suspension A, stir for 30 min to obtain a uniform suspension B;
[0104] Step 3: While magnetically stirring, add 0.08 mmol (0.009 g) of NH4VO3 powder to the above suspension B, and stir for 30 min to obtain a well-mixed reaction precursor solution C;
[0105] Step 4: Transfer the precursor solution C to a hydrothermal reactor with a filling ratio of 80% and react at 210℃ for 18 hours. After the reaction, wash the resulting precipitate three times with deionized water and anhydrous ethanol, and dry it at 80℃ for 10 hours to obtain BiO(IO3). 0.94 (VO3) 0.06 Photocatalyst powder.
[0106] Figure 1 The BiO(IO3) prepared in this invention 1-x (VO3) xThe XRD patterns of the photocatalyst powder are shown in the figure. Curves a and b represent the XRD patterns of the photocatalyst powders prepared in Comparative Example 1 and Examples 1-3, respectively. The diffraction peaks at diffraction angles 2θ = 8.2°, 27.5°, 31.3°, 31.7°, 32.6°, 33.0°, 45.2°, 45.8°, 53.4°, 53.9°, 55.0°, and 56.7° correspond to the (010), (121), (002), (200), (040), (131), (042), (240), (123), (321), (161), and (242) crystal planes of BiOIO3 (mp-1191266), respectively. It belongs to the orthorhombic crystal system, space group Pca21, and cell parameters are: α = 90.00°, β = 90.00°, γ = 90.00°. Compared with BiOIO3, the prepared BiO(IO3) 1-x (VO3) x The diffraction peak intensity of VO3 first increases and then decreases with increasing doping concentration, indicating that VO3 - The introduction of functional groups can affect the crystallinity of photocatalyst powders. (BiO(IO3)) 0.96 (VO3) 0.04 The diffraction peak intensity is the lowest, which is related to the increase in the defect concentration in its lattice.
[0107] Figure 2 The BiO(IO3) prepared in this invention 1-x (VO3) x The XRD patterns of the photocatalyst powder show magnified diffraction peaks in the 26.5°–28.5° range. In the figure, curves a and b represent the magnified XRD diffraction peaks of the photocatalyst powders prepared in Comparative Example 1 and Examples 1–3, respectively, in the 26.5°–28.5° range. As can be seen from the figure, the introduction of VO3 into the BiOIO3 lattice… - Following the group, the diffraction peak of its (121) crystal plane shifts towards higher angles. According to Bragg's equation: 2dsinθ=nλ, the diffraction angle 2θ shifts towards higher angles, and the interplanar spacing d of the surface decreases. V 5+ The radius of the ion is approximately 0.054 nm, I 5+ The radius of the ion is approximately 0.094 nm, V 5+ The radius of the ion is significantly smaller than that of I. 5+ Therefore, the XRD diffraction peaks shift towards higher angles, indicating small-radius VO3+ ions. - Ionic groups were successfully introduced into the lattice of BiOIO3, and they occupied a large radius of IO3. - Lattice sites of ionic groups.
[0108] Figure 3The BiO(IO3) prepared in this invention 1-x (VO3) x The FT-IR spectra of the photocatalyst powder are shown in the figure. Curves a and b represent the FT-IR spectra of the photocatalyst powders prepared in Comparative Example 1 and Examples 1-3, respectively. The prepared photocatalyst powders exhibit FT-IR spectra at 511 cm⁻¹. -1 The characteristic peak at 678 cm⁻¹ corresponds to the Bi-O vibration, and it is located at 678 cm⁻¹. -1 and 774cm -1 The two relatively strong characteristic peaks at 1396 cm⁻¹ correspond to the stretching vibrations of the IO bond. -1 The characteristic peak at that location is attributed to NO3 introduced during the preparation of the photocatalyst powder. - Impurity ions, 3135 cm -1 The characteristic peak at that point corresponds to the stretching vibration of the OH bond in the adsorbed water molecule.
[0109] Figure 4 The BiO(IO3) prepared in this invention 1-x (VO3) x The FT-IR spectrum of photocatalyst powder at 700 cm⁻¹ -1 -800cm -1 The characteristic absorption peaks amplified within the range are shown in the figure. Curves a and b represent the amplified FT-IR characteristic absorption peaks of the photocatalyst powders prepared in Comparative Example 1 and Examples 1-3, respectively. VO3 - The introduction of ionic groups into the BiOIO3 lattice alters its chemical environment. Therefore, compared to BiOIO3, BiO(IO3)... 1-x (VO3) x The stretching vibration peaks of the IO bonds in the crystal lattice are significantly shifted towards lower wavenumbers.
[0110] Figure 5 The BiO(IO3) prepared in this invention 1-x (VO3) x The Raman spectra of the photocatalyst powders are shown in the figure. Curves a and c represent the Raman spectra of the photocatalyst powders prepared in Comparative Example 1 and Example 2, respectively. For BiOIO3, four characteristic peaks can be detected in its Raman spectrum, located at 164 cm⁻¹. -1 681cm -1 707cm -1 and 774cm -1 Introducing VO3 into the lattice of BiOIO3. - The Raman spectrum of the catalyst powder changed significantly after the addition of ionic groups. In addition to the four Raman characteristic peaks mentioned above, BiO(IO3) also showed changes. 0.96 (VO3) 0.04Additional characteristic peaks can be detected in the Raman spectrum. As shown in the figure, it is located at 327 cm⁻¹. -1 371cm -1 740cm -1 and 825cm -1 The characteristic peaks at these locations correspond to the asymmetric and symmetric bending modes and the asymmetric and symmetric stretching modes of the VO3 bond, respectively, further indicating that VO3... - Ionic groups were successfully introduced into the BiOIO3 lattice. And BiO(IO3) 0.96 (VO3) 0.04 The Raman peak intensity of VO3 is significantly higher than that of BiOIO3, a phenomenon also attributed to VO3. - Changes in the chemical environment of the crystal structure caused by doping.
[0111] Figure 6 The BiO(IO3) prepared in this invention 1-x (VO3) x SEM images of the photocatalyst powders, Figures a and b respectively showing the SEM images of the photocatalyst powders prepared in Comparative Example 1 and Examples 1-3. Figure 6 As shown in Figure a, the BiOIO3 photocatalyst prepared in Comparative Example 1 exhibits a thin, irregular nanosheet morphology with a thickness of approximately 5 nm. Figure 6 As shown in b, the BiO(IO3) prepared in Example 1 0.98 (VO3) 0.02 The photocatalyst exhibits a smooth nanoribbon morphology with a thickness of approximately 12 nm. For example... Figure 6 As shown in Figure c, the BiO(IO3) prepared in Example 2 0.96 (VO3) 0.04 The photocatalyst exhibits a nanoribbon morphology with serrated edges, and small, irregular nanosheets are attached to the surface of the nanoribbons. The nanoribbon thickness is approximately 12 nm, and the nanosheet thickness is approximately 6 nm. Figure 6 As shown in d, the BiO(IO3) prepared in Example 3 0.94 (VO3) 0.06 It exhibits a smooth surface morphology of nanoribbons and nanosheets, with irregular nanoparticles attached to the surface. The thickness of the nanorods and nanosheets is approximately 13 nm.
[0112] Figure 7 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 Elemental mapping diagram of photocatalyst powder. As shown in the diagram, BiO(IO3)... 0.96 (VO3) 0.04 Composed of Bi, O, I, and V elements, with I accounting for approximately 4.24 wt% by mass, further indicating that VO3- Ionic groups were successfully introduced into the BiOIO3 lattice, consistent with FT-IR and Raman test results.
[0113] Figure 8 The BiO(IO3) prepared in this invention 1-x (VO3) x The EPR spectra of the photocatalyst powders are shown. In the figure, curves a and c are the EPR spectra of the photocatalyst powders prepared in Comparative Example 1 and Example 2, respectively. (BiOIO3 and BiO(IO3)) 0.96 (VO3) 0.04 Both showed detectable EPR signals with a g value of approximately 2.006, corresponding to single-electron capture at oxygen vacancy sites, indicating that BiOIO3 and BiO(IO3) were involved. 0.96 (VO3) 0.04 Oxygen vacancy defects are present in all crystal lattices. Furthermore, the BiO(IO3) prepared in Example 2... 0.96 (VO3) 0.04 The EPR signal of the photocatalyst powder is significantly stronger than that of BiOIO3, indicating that BiO(IO3) has a stronger EPR signal. 0.96 (VO3) 0.04 The oxygen vacancy concentration in the crystal lattice is higher than that in BiOIO3, i.e., VO3. - The introduction of ionic groups is conducive to the formation of oxygen vacancies.
[0114] Figure 9 The BiO(IO3) prepared in this invention 1-x (VO3) x High-resolution XPS Bi 4f spectra of photocatalyst powders are shown. In the figure, curves a and c are the high-resolution XPS Bi 4f spectra of the photocatalyst powders prepared in Comparative Example 1 and Example 2, respectively. In the high-resolution XPS Bi 4f spectra of BiOIO3, the characteristic peaks located at 159.18 eV and 164.48 eV correspond to Bi, respectively. 3+ 4f 7 / 2 and 4f 5 / 2 Orbit. BiO(IO3) 0.96 (VO3) 0.04 The two characteristic peaks mentioned above are located at 158.98 eV and 164.28 eV, respectively, indicating the introduction of VO3 into the BiOIO3 lattice. - The binding energy of Bi decreases after the addition of ionic groups, indicating an increase in its charge density.
[0115] Figure 10 The BiO(IO3) prepared in this invention 1-x (VO3) xHigh-resolution XPS 1s spectra of the photocatalyst powder are shown. In the figure, curves a and c are the high-resolution XPS 1s spectra of the photocatalyst powders prepared in Comparative Example 1 and Example 2, respectively. The characteristic peaks at 530.54 eV and 530.08 eV are attributed to lattice oxygen atoms. (BiO(IO3)) 0.96 (VO3) 0.04 The binding energy of oxygen atoms in the lattice is significantly lower than that of BiOIO3, indicating that the charge density of oxygen atoms in BiOIO3 is higher than that in BiOIO3.
[0116] Figure 11 The BiO(IO3) prepared in this invention 1-x (VO3) x High-resolution XPS I 3d spectra of photocatalyst powders are shown. In the figure, curves a and c are the high-resolution XPS I 3d spectra of the photocatalyst powders prepared in Comparative Example 1 and Example 2, respectively. For BiOIO3, the two strong characteristic peaks at 623.99 eV and 635.49 eV correspond to I, respectively. 5+ 3d ions 5 / 2 and 3D 3 / 2 The orbitals, with their two relatively weak characteristic peaks at 619.08 eV and 630.68 eV, correspond to I, respectively. - 3D 5 / 2 and 3D 3 / 2 Orbit. For BiO(IO3) 0.96 (VO3) 0.04 I 5+ 3D 5 / 2 and 3D 3 / 2 The characteristic peaks of the orbital shifted to 623.78 eV and 635.18 eV, while I - 3D 5 / 2 and 3D 3 / 2 The characteristic peaks of the orbitals shifted to 618.78 eV and 630.36 eV. The shift of the characteristic peaks of element I towards lower binding energies indicates an increase in its charge density.
[0117] Depend on Figures 9-11 Analysis shows that BiO(IO3) 0.96 (VO3) 0.04 In the crystal lattice, the charge densities of Bi, O, and I are all greater than those of BiOIO3, a phenomenon attributed to the increased oxygen vacancy concentration. Positively charged oxygen vacancy sites typically bind localized electrons to maintain the charge balance of the entire material system. (BiO(IO3)) 0.96 (VO3) 0.04 The oxygen vacancy concentration in the crystal lattice is higher than that in BiOIO3, i.e., BiO(IO3). 0.96 (VO3) 0.04The higher concentration of localized electrons bound in the crystal lattice leads to an increase in the charge density of Bi, O, and I elements.
[0118] Figure 12 The BiO(IO3) prepared in this invention 1-x (VO3) x The N2 adsorption-desorption isotherms of the photocatalyst powder are shown in the figure. Curves a and b represent the N2 adsorption-desorption isotherms of the photocatalyst powders prepared in Comparative Example 1 and Examples 1-3, respectively. As can be seen from the figure, the BiO(IO3) prepared in this invention... 1-x (VO3) x The photocatalyst powder exhibits a type IV isotherm curve, with its hysteresis loop extending from P / P0 = 0.05 to P / P0 = 1, indicating that the photocatalyst powder prepared in this invention is a mesoporous and microporous material. The prepared photocatalyst powder possesses a nanosheet stacked morphology, which is the main reason for the formation of the porous structure. The prepared BiOIO3 and BiO(IO3) materials... 0.98 (VO3) 0.02 BiO(IO3) 0.96 (VO3) 0.04 And BiO(IO3) 0.94 (VO3) 0.06 The BET specific surface area of the photocatalyst powder is 5.455 m². 2 ·g -1 12.402m 2 ·g -1 25.617m 2 ·g -1 and 7.123m 2 ·g -1 VO3 - The introduction of ionic groups increases the BET specific surface area of the photocatalyst powder, providing more active sites for the photocatalytic reaction. (BiO(IO3)) 0.96 (VO3) 0.04 The BET has the largest specific surface area, which is related to the formation of its serrated edge structure.
[0119] Figure 13 The BiO(IO3) prepared in this invention 1-x (VO3) x The pore size distribution curves of the photocatalyst powders are shown in the figure. Curves a and b represent the pore size distribution curves of the photocatalyst powders prepared in Comparative Example 1 and Examples 1-3, respectively. (BiOIO3, BiO(IO3)) 0.98 (VO3) 0.02 BiO(IO3) 0.96 (VO3) 0.04 And BiO(IO3) 0.94(VO3) 0.06 The total pore volume is 0.01589 cm³. 3 ·g -1 0.07771cm 3 ·g -1 0.1505cm 3 ·g -1 and 0.02856cm 3 ·g -1 The average pore sizes were 15.234 nm, 17.760 nm, 19.214 nm, and 17.867 nm, respectively, further indicating that the photocatalyst powder prepared in this invention is a mesoporous and microporous material, consistent with the test results of the N2 adsorption-desorption isotherm curve. Example 2: BiO(IO3) prepared. 0.96 (VO3) 0.04 Photocatalyst powder has the largest total pore volume and average pore size, which is beneficial to the adsorption of reactants and the migration of products.
[0120] Figure 14 The BiO(IO3) prepared in this invention 1-x (VO3) x The UV-Vis diffuse reflectance spectra of the photocatalyst powders are shown in the figure. Curves a and b represent the UV-Vis diffuse reflectance spectra of the photocatalyst powders prepared in Comparative Example 1 and Examples 1-3, respectively. The light absorption edge of BiOIO3 is located at approximately 450 nm, meaning that the light absorption edge of the BiOIO3 photocatalyst powder prepared in this invention is in the visible light range. This has certain advantages compared to BiOIO3 photocatalysts reported in the literature that only respond to UV light. Furthermore, a weak Urbach tail absorption can be observed near the light absorption edge of BiOIO3, a phenomenon attributed to the formation of oxygen vacancy-induced defect states. VO3 - The introduction of ionic groups will lead to an increase in the oxygen vacancy concentration in the BiOIO3 lattice, and the oxygen vacancy-induced defect state density will also increase accordingly; in addition, VO3 - Ionic groups can also induce the formation of defect states. Therefore, the BiO(IO3) prepared in this invention... 1-x (VO3) x The light absorption intensity of the photocatalyst powder in the 360nm-800nm range is significantly higher than that of BiOIO3, i.e., VO3. - The introduction of ionic groups broadens the photoresponse range of BiOIO3 and improves its utilization of solar energy.
[0121] Figure 15 The BiO(IO3) prepared in this invention 1-x (VO3) xThe Kubelka-Munk conversion curves of the UV-Vis diffuse reflectance spectra of the photocatalyst powder are shown in the figure. Curves a and b represent the Kubelka-Munk conversion curves of the UV-Vis diffuse reflectance spectra of the photocatalyst powders prepared in Comparative Example 1 and Examples 1-3, respectively. Based on the Kubelka-Munk conversion formula, the prepared BiOIO3 and BiO(IO3) can be calculated. 0.98 (VO3) 0.02 BiO(IO3) 0.96 (VO3) 0.04 And BiO(IO3) 0.94 (VO3) 0.06 The band gaps are 2.78 eV, 2.30 eV, 2.06 eV, and 2.56 eV, respectively, which means that VO3 is introduced... - Ionic groups can significantly reduce the band gap of BiO(IO3), as seen in the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 The photocatalyst powder has the smallest band gap. Furthermore, the BiO(IO3) prepared in this invention... 1-x (VO3) x The additional band gap energy in the Kubelka-Munk conversion curve of the photocatalyst powder is attributed to oxygen vacancies and VO3. - The formation of defect states induced by impurity ions, located at the bottom of the conduction band of the photocatalyst powder. Calculations show that BiOIO3 and BiO(IO3)... 0.98 (VO3) 0.02 BiO(IO3) 0.96 (VO3) 0.04 And BiO(IO3) 0.94 (VO3) 0.06 The defect states can extend to the bottom of the conduction band at 1.10 eV, 0.34 eV, 0.18 eV, and 0.62 eV, respectively. The calculation results show that deep trapped states induced by defects are formed in the band gap of BiOIO3, while BiO(IO3)... 0.98 (VO3) 0.02 BiO(IO3) 0.96 (VO3) 0.04 And BiO(IO3) 0.94 (VO3) 0.06 The band gap forms a shallow trapped state induced by defects; the deep trapped state induced by defects becomes the recombination center of photogenerated carriers, while the shallow trapped state can serve as a springboard for photogenerated electron transitions to promote electron-hole pair separation, which is beneficial to improving photocatalytic activity.
[0122] Figure 16 The BiO(IO3) prepared in this invention 1-x(VO3) x The degradation curves of photocatalyst powder on tetracycline hydrochloride under ultraviolet light irradiation are shown in the figure. Curves a and b represent the degradation curves of photocatalyst powder prepared in Comparative Example 1 and Examples 1-3 on tetracycline hydrochloride under ultraviolet light irradiation, respectively. The initial concentration of tetracycline hydrochloride was 20 mg·L⁻¹. -1 The catalyst dosage during the reaction was 40 mg, the contaminant solution dosage was 40 mL, and the light source used was a 500 W mercury lamp. As can be seen from the figure, BiO(IO3) 1-x (VO3) x The degradation activity of BiO(IO3) against tetracycline under ultraviolet light irradiation was significantly higher than that of BiOIO3. After 40 min of ultraviolet light irradiation, the degradation efficiency of BiO(IO3) against tetracycline was 66.29%, compared with the BiO(IO3) prepared in Examples 1-3. 1-x (VO3) x The photocatalysts showed degradation efficiencies of 88.52%, 94.14%, and 92.64% for tetracycline, respectively. The BiO(IO3) prepared in Example 2... 0.96 (VO3) 0.04 The photocatalyst powder exhibits the highest degradation activity for tetracycline.
[0123] Figure 17 The BiO(IO3) prepared in this invention 1-x (VO3) x The kinetic curves of photocatalytic degradation of tetracycline hydrochloride by photocatalyst powder under ultraviolet light irradiation are shown in the figure. Curves a and b represent the kinetic curves of photocatalyst powder prepared in Comparative Example 1 and Examples 1-3, respectively, under ultraviolet light irradiation for the photocatalyst degradation of tetracycline. As shown in the figure, under ultraviolet light irradiation, BiOIO3 and BiO(IO3) 0.98 (VO3) 0.02 BiO(IO3) 0.96 (VO3) 0.04 BiO(IO3) 0.94 (VO3) 0.06 The degradation rate of tetracycline was 0.0266 min. -1 0.0526min -1 0.0862min -1 and 0.0618min -1 The BiO(IO3) prepared in Example 2 0.96 (VO3) 0.04 The photocatalyst exhibited the highest degradation rate for tetracycline, which was 3.24 times that of BiOIO3.
[0124] Figure 18 The BiO(IO3) prepared in this invention 1-x (VO3)x The degradation curves of photocatalyst powder on tetracycline hydrochloride under simulated sunlight irradiation are shown in the figure. Curves a and b represent the degradation curves of photocatalyst powder prepared in Comparative Example 1 and Examples 1-3 on tetracycline hydrochloride under simulated sunlight irradiation, respectively. The initial concentration of tetracycline was 20 mg·L⁻¹. -1 The catalyst dosage during the reaction was 40 mg, the contaminant solution dosage was 40 mL, and the light source used was a 500 W xenon lamp. As can be seen from the figure, the BiO(IO3) prepared in this invention... 1-x (VO3) x The photocatalyst also showed higher activity than BiOIO3 in degrading tetracycline under simulated sunlight irradiation. (BiO(IO3) prepared in Example 2) 0.96 (VO3) 0.04 The photocatalyst exhibited the highest degradation activity for tetracycline; after 60 minutes of simulated sunlight irradiation, BiO(IO3) showed the highest degradation activity. 0.96 (VO3) 0.04 The photocatalyst achieved a tetracycline degradation efficiency of 95.22%, which is 1.64 times that of BiOIO3 (58.01%) under the same conditions.
[0125] Figure 19 The BiO(IO3) prepared in this invention 1-x (VO3) x The kinetic curves of photocatalytic degradation of tetracycline by photocatalyst powder under simulated sunlight irradiation are shown in the figure. Curves a and b represent the kinetic curves of photocatalyst powder prepared in Comparative Example 1 and Examples 1-3, respectively, under simulated sunlight irradiation for the photocatalyst degradation of tetracycline. Under simulated sunlight irradiation, BiOIO3 and BiO(IO3) 0.98 (VO3) 0.02 BiO(IO3) 0.96 (VO3) 0.04 And BiO(IO3) 0.94 (VO3) 0.06 The degradation rate of tetracycline was 0.0113 min. -1 0.0169min -1 0.0396min -1 and 0.0237min -1 The BiO(IO3) prepared in Example 2 0.96 (VO3) 0.04 The photocatalyst exhibited the highest degradation rate for tetracycline, which was 3.50 times that of BiOIO3.
[0126] Figure 20 The BiO(IO3) prepared in this invention 1-x (VO3) xThe degradation curves of ciprofloxacin by photocatalyst powder under simulated sunlight irradiation are shown in the figure. Curves a and b represent the degradation curves of ciprofloxacin by the photocatalyst powder prepared in Comparative Example 1 and Examples 1-3, respectively. The initial concentration of ciprofloxacin was 10 mg·L⁻¹. -1 During the reaction, the catalyst dosage was 40 mg, the contaminant solution dosage was 40 mL, and the light source used was a 500 W xenon lamp. It can be clearly seen from the figure that the BiO(IO3) prepared in this invention... 1-x (VO3) x The photocatalyst exhibited higher degradation activity for ciprofloxacin than BiOIO3 under simulated sunlight irradiation. After 60 minutes of simulated sunlight irradiation, the degradation efficiency of BiOIO3 for ciprofloxacin was 49.84%, compared to the BiO(IO3) prepared in Examples 1-3. 0.98 (VO3) 0.02 BiO(IO3) 0.96 (VO3) 0.04 And BiO(IO3) 0.94 (VO3) 0.06 The degradation efficiencies of ciprofloxacin were 69.44%, 92.04%, and 80.49%, respectively, which were 1.85-1.39 times that of BiOIO3.
[0127] Figure 21 The BiO(IO3) prepared in this invention 1-x (VO3) x The kinetic curves of photocatalytic degradation of ciprofloxacin by photocatalyst powder under simulated sunlight irradiation are shown in the figure. Curves a and b represent the kinetic curves of photocatalyst powder prepared in Comparative Example 1 and Examples 1-3, respectively, under simulated sunlight irradiation for the photocatalyst degradation of ciprofloxacin. It can be seen from the figure that the degradation rate of ciprofloxacin by BiOIO3 under simulated sunlight irradiation is 0.0092 min. -1 BiO(IO3) prepared in Examples 1-3 1-x (VO3) x The degradation rate of ciprofloxacin by the photocatalyst powder increased to 0.0196 min. -1 0.0394min -1 and 0.0254min -1 These figures are 2.13 times, 4.28 times, and 2.76 times that of BiOIO3, respectively.
[0128] Figure 22 The BiO(IO3) prepared in this invention 1-x (VO3) xThe TOC removal rates of photocatalyst powder during the degradation of tetracycline hydrochloride and ciprofloxacin under simulated sunlight irradiation are shown in bars a and b, respectively. Bars c and d represent the TOC removal rates of photocatalyst powder prepared in Example 2 and Comparative Example 1 during the degradation of tetracycline hydrochloride under simulated sunlight irradiation. After 60 min of simulated sunlight irradiation, the TOC removal rates of BiO(IO3)3 photocatalytic degradation of tetracycline hydrochloride and ciprofloxacin were 30.69% and 36.81%, respectively. Under the same reaction conditions, the TOC removal rates of BiO(IO3)3 prepared in Comparative Example 2 were also shown. 0.96 (VO3) 0.04 The photocatalyst powder achieved TOC removal rates of 82.64% and 87.31% respectively during the photocatalytic degradation of tetracycline hydrochloride and ciprofloxacin. During the photocatalytic reaction, BiO(IO3)... 0.96 (VO3) 0.04 The TOC removal rate of the degraded tetracycline hydrochloride and ciprofloxacin was significantly higher than that of BiOIO3, indicating that the BiO(IO3) prepared in this invention... 1-x (VO3) x The photocatalyst powder exhibits high mineralization capacity for tetracycline hydrochloride and ciprofloxacin under simulated sunlight irradiation.
[0129] Figure 23 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 Degradation curves of photocatalyst powder on antibiotics such as oxytetracycline, ofloxacin, norfloxacin, and metronidazole under simulated sunlight irradiation. The initial concentrations of oxytetracycline, ofloxacin, norfloxacin, and metronidazole were all 20 mg·L⁻¹. -1 During the photocatalytic reaction, the catalyst dosage was 40 mg, the pollutant solution dosage was 40 mL, and the light source was a 500 W xenon lamp. After simulating sunlight irradiation for 90 min, BiO(IO3) 0.96 (VO3) 0.04 The degradation efficiencies for tetracycline, ofloxacin, norfloxacin, and metronidazole were 89.62%, 86.44%, 79.07%, and 64.83%, respectively. These test results indicate that the BiO(IO3) prepared in this invention... 1-x (VO3) x Photocatalyst powders do not exhibit selectivity in the photodegradation of antibiotics.
[0130] Figure 24 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04The kinetic curves of the photocatalytic degradation of tetracycline, ofloxacin, norfloxacin, and metronidazole by the photocatalyst powder under simulated sunlight irradiation are shown in the figure. As can be seen from the figure, BiO(IO3) 0.96 (VO3) 0.04 Under simulated sunlight irradiation, the degradation rates of tetracycline, ofloxacin, norfloxacin, and metronidazole were 0.0322 min. -1 0.0212min -1 0.0168min -1 and 0.0108min -1 .
[0131] Figure 25 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 The TOC removal rate of photocatalyst powder during simulated sunlight irradiation for the degradation of tetracycline, ofloxacin, norfloxacin, and metronidazole. After 90 min of simulated sunlight irradiation, the TOC removal rate of BiO(IO3) was [data missing]. 0.96 (VO3) 0.04 The photocatalytic degradation of tetracycline, ofloxacin, norfloxacin, and metronidazole by the photocatalyst achieved TOC removal rates of 83.46%, 85.77%, 75.42%, and 61.49%, respectively. These results indicate that the BiO(IO3) prepared in this invention... 1-x (VO3) x Photocatalyst powders also exhibit high mineralization capacity for antibiotics such as tetracycline, ofloxacin, norfloxacin, and metronidazole under simulated sunlight irradiation.
[0132] Figure 26 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 The results of a cyclic experiment on the photocatalytic degradation of tetracycline hydrochloride by photocatalyst powder under simulated sunlight irradiation. As can be seen from the figure, during the first to sixth cycles, after 60 minutes of simulated sunlight irradiation, the BiO(IO3) prepared in Example 2 showed... 0.96 (VO3) 0.04 The photocatalysts exhibited degradation efficiencies of 95.22%, 92.24%, 87.69%, 93.16%, 84.19%, and 85.97% for tetracycline, respectively; during the cyclic reaction, BiO(IO3)... 0.96 (VO3) 0.04 The degradation efficiency of tetracycline remained basically stable, proving that the BiO(IO3) prepared in this invention... 1-x (VO3) x Photocatalysts exhibit good cycle stability.
[0133] Figure 27It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 XRD patterns of the photocatalyst powder before and after the cyclic reaction. The figures show that after six cycles, BiO(IO3)... 0.96 (VO3) 0.04 The XRD pattern did not change significantly, indicating that the BiO(IO3) prepared in this invention... 1-x (VO3) x Photocatalysts exhibit good structural stability.
[0134] Figure 28 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 The UV-Vis diffuse reflectance spectra of the photocatalyst powder before and after the cyclic reaction are shown in the figure. Curves a and b represent the UV-Vis diffuse reflectance spectra of the photocatalyst powder prepared in Example 2 before and after the cyclic reaction, respectively. It can be clearly seen from the figure that after the cyclic reaction, BiO(IO3)... 0.96 (VO3) 0.04 The light absorption intensity is significantly enhanced in the 440nm-800nm range. This invention prepares BiO(IO3) via an HNO3-assisted hydrothermal reaction. 1-x (VO3) x BiO(IO3) was prepared from photocatalyst powder under acidic reaction conditions. 1-x (VO3) x The surface of the photocatalyst powder adsorbs a large amount of H + Ions, surface adsorption of H + The presence of ions weakens the Bi-O bond. Simulated sunlight contains 4%-5% ultraviolet light. During the photocatalytic reaction, BiO(IO3) undergoes high-energy ultraviolet radiation. 1-x (VO3) x Oxygen escapes from the surface lattice, leading to an increase in the oxygen vacancy concentration within the lattice, which in turn enhances its light absorption in the 440nm-800nm range. This phenomenon is beneficial to BiO(IO3). 1-x (VO3) x Further improvement in photocatalytic performance.
[0135] Figure 29 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 The EPR spectra of the photocatalyst powder before and after the cyclic reaction are shown in the figure. Curves a and b represent BiO(IO3) and IO3, respectively. 0.96 (VO3) 0.04EPR spectra of the photocatalyst before and after cycling. After six cycles, BiO(IO3) 0.96 (VO3) 0.04 The significantly enhanced EPR signal indicates an increased oxygen vacancy concentration in its lattice, consistent with the results of UV-Vis diffuse reflectance spectroscopy.
[0136] Figure 30 The BiO(IO3) prepared in this invention 1-x (VO3) x The transient photocurrent response curves of the photocatalyst powder under simulated sunlight irradiation are shown in the figure. Curves a and b represent the transient photocurrent response curves of the photocatalyst powders prepared in Comparative Example 1 and Examples 1-3, respectively, under simulated sunlight irradiation. During the test, 0.1 mol·L⁻¹ -1 A Na₂SO₄ solution was used as the electrolyte, and a 300W xenon lamp was used as the light source. Under simulated sunlight irradiation, BiOIO₃ and BiO(IO₃) 0.98 (VO3) 0.02 BiO(IO3) 0.96 (VO3) 0.04 And BiO(IO3) 0.94 (VO3) 0.06 The transient photocurrent values were 0.4162 μA, 2.098 μA, 2.995 μA, and 1.418 μA, respectively. The BiO(IO3) prepared in this invention... 1-x (VO3) x The transient photocurrent value of the photocatalyst is significantly higher than that of BiOIO3, as shown in Example 2 with BiO(IO3). 0.96 (VO3) 0.04 The transient photocurrent of the photocatalyst under simulated sunlight irradiation is 7.20 times that of BiOIO3, indicating that the BiO(IO3) prepared in this invention... 1-x (VO3) x The photocatalyst powder exhibits higher separation efficiency of photogenerated electron-hole pairs than BiOIO3 under simulated sunlight irradiation.
[0137] Figure 31 The BiO(IO3) prepared in this invention 1-x (VO3) x Electrochemical impedance spectroscopy (EIS) spectra of photocatalyst powder under simulated sunlight irradiation are shown in the figure. Curves a and b represent the EIS spectra of the photocatalyst powders prepared in Comparative Example 1 and Examples 1-3, respectively, under simulated sunlight irradiation. The obtained Nyquist plots were fitted using ZSimpWin software, with R being the selected equivalent simulation circuit. s (C sc R ct (Cedl R a ), where R s C sc R ct C edl and R a These represent solution resistance, space charge capacitance, charge transfer resistance, electrochemical double-layer capacitance, and electrolyte resistance, respectively. As shown in the figure, BiOIO3 and BiO(IO3) 0.98 (VO3) 0.02 BiO(IO3) 0.96 (VO3) 0.04 And BiO(IO3) 0.94 (VO3) 0.06 The charge transfer resistances of BiO(IO3) are 170.3 kΩ, 88.11 kΩ, 47.80 kΩ and 65.74 kΩ, respectively. 1-x (VO3) x The charge transfer resistance of the photocatalyst is significantly lower than that of BiOIO3, indicating that VO3 - The introduction of ionic groups helps to separate and transfer photogenerated carriers, thereby improving the separation efficiency of photogenerated electron-hole pairs.
[0138] Figure 32 The BiO(IO3) prepared in this invention 1-x (VO3) x The photoluminescence spectra of the photocatalyst powder in the 330nm-600nm range are shown in the figure. Curves a and c represent the photoluminescence spectra of the photocatalyst powders prepared in Comparative Example 1 and Example 2, respectively, in the 330nm-600nm range, with an excitation wavelength of 310nm. (BiOIO3 and BiO(IO3)) 0.96 (VO3) 0.04 A distinct fluorescence emission peak could be detected in the 400nm-550nm range, corresponding to conduction band electrons and defects (I0). - The recombination of photogenerated electrons trapped in the shallow trapped state with valence band holes (induced by oxygen vacancies) is significant. The fluorescence emission peak of BiOIO3 is significantly stronger than that of BiO(IO3). 0.96 (VO3) 0.04 This indicates that the recombination rate of photogenerated electron-hole pairs in BiOIO3 is relatively high, i.e., VO3 - The introduction of ionic groups can improve the separation efficiency of photogenerated electron-hole pairs.
[0139] Figure 33 The BiO(IO3) prepared in this invention 1-x (VO3) xThe photoluminescence spectra of the photocatalyst powder in the 580 nm-700 nm range are shown. Curves a and c are the photoluminescence spectra of the photocatalyst powders prepared in Comparative Example 1 and Example 2, respectively, with an excitation wavelength of 310 nm. BiOIO3 and BiO(IO3) 0.96 (VO3) 0.04 The fluorescence emission peak in the 610nm-680nm range is attributed to defects (I0.05). - (and oxygen vacancies) induce recombination between photogenerated electrons trapped in the deep-trapped state and valence band holes. Figure 14 and Figure 15 The test results and analysis show that for BiOIO3, by I - The defect level induced by oxygen vacancies can extend to the bottom of the conduction band at 1.10 eV. The formation of defect-induced deep trapped states serves as a recombination center for photogenerated carriers, resulting in a high recombination rate of photogenerated electron-hole pairs in BiOIO3. Therefore, BiOIO3 exhibits a strong fluorescence emission peak in the 610 nm-680 nm range; while BiO(IO3) 0.96 (VO3) 0.04 The defect energy level can only extend to the bottom of the conduction band at 0.18 eV. The relaxation of photogenerated electrons to the defect state can suppress the recombination of photogenerated carriers, resulting in a weaker fluorescence emission peak in the range of 610 nm-680 nm, which corresponds to a higher separation efficiency of photogenerated carriers.
[0140] Figure 34 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 The results of the photocatalytic degradation of tetracycline hydrochloride by photocatalyst powder under simulated sunlight irradiation show the active species capture experiment. In the figure, curve a represents the control group, and curves bd represent BiO(IO3) after the introduction of p-benzoquinone, sodium oxalate, and tert-butanol. 0.96 (VO3) 0.04 Degradation curves of tetracycline, p-benzoquinone, sodium oxalate, and tert-butanol were used as superoxide radicals (·O2). - ), hole (h + It acts as a scavenger of hydroxyl radicals (·OH). After introducing p-benzoquinone, sodium oxalate, and tert-butanol, under the same reaction conditions, BiO(IO3)... 0.96 (VO3) 0.04 The degradation efficiency of tetracycline decreased from 95.22% to 39.35%, 49.50%, and 53.96%, respectively, indicating that under simulated sunlight irradiation, vacuoles and hydroxyl radicals are the main active species playing a major role in the degradation of tetracycline, while superoxide radicals are the secondary active species.
[0141] Figure 35The figure shows the Mott-Schottky curve of the BiOIO3 photocatalyst powder prepared in Comparative Example 1. As can be seen from the figure, the linear portion of the BiOIO3 Mott-Schottky curve exhibits a negative slope, indicating that BiOIO3 is an n-type semiconductor. By fitting its linear portion, the flat band potential of BiOIO3 is found to be -0.30 eV. For an n-type semiconductor, its flat band is located approximately 0.1 eV below the inverted band. Therefore, the conduction band potential of BiOIO3 is approximately -0.40 eV. According to E... g =E VB -E CB The valence band potential of BiOIO3 was calculated to be +2.38 eV.
[0142] Figure 36 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 Mott-Schottky curves of photocatalyst powders. As shown in the figure, BiO(IO3)... 0.96 (VO3) 0.04 The linear portion of the Mott-Schottky curve also has a negative slope, indicating that BiO(IO3) 0.96 (VO3) 0.04 Also an n-type semiconductor, namely VO3 - The introduction of ionic groups did not change the semiconductor type. (For BiO(IO3)) 0.96 (VO3) 0.04 The linear portion of the Mott-Schottky curve was fitted to obtain BiO(IO3). 0.96 (VO3) 0.04 Its flat band potential is -0.56 eV, and its conduction band potential is -0.66 eV. BiO(IO3) 0.96 (VO3) 0.04 The conduction band position is higher than that of BiOIO3, a phenomenon attributed to VO3. - Doping increases the oxygen vacancy concentration. This increased oxygen vacancy concentration leads to a large number of free electrons in BiO(IO3). 0.96 (VO3) 0.04 Accumulation in the crystal lattice leads to an uplift of its conduction band position, enhancing the reduction capability of photogenerated electrons. According to E... g =E VB -E CB The BiO(IO3) was calculated. 0.96 (VO3) 0.04 Its valence potential is +1.40 eV.
[0143] Figure 37 The BiO(IO3) prepared in this invention 1-x (VO3) xThe photocatalytic mechanism of the photocatalyst under simulated sunlight irradiation. Based on the above test results and analysis, it can be seen that introducing VO3 into the BiOIO3 lattice... - After the addition of ionic groups, its band gap decreased from 2.78 eV to 2.06 eV (BiO(IO3)). 0.96 (VO3) 0.04 ), i.e., VO3 - The introduction of ionic groups improves the utilization rate of solar energy in BiOIO3. Furthermore, VO3... - The introduction of ionic groups and the formation of serrated edges lead to an increase in the oxygen vacancy concentration in the photocatalyst powder lattice. A large number of localized electrons accumulate at the oxygen vacancy sites, resulting in BiO(IO3) 0.96 (VO3) 0.04 The conduction band position of the photocatalyst powder increased from -0.40 eV to -0.66 eV, improving the reduction ability of photogenerated electrons. As shown in the figure, under simulated sunlight irradiation, BiO(IO3) 0.96 (VO3) 0.04 Electrons and holes are generated upon excitation; furthermore, localized electrons in defect states interact with incident photons to produce high-energy hot electrons. (BiO(IO3)) 0.96 (VO3) 0.04 Conduction band electrons and high-energy hot electrons react with O2 adsorbed on the catalyst surface to generate ·O2. - Free radicals, ·O2 - The free radical further reacts with electrons to generate H₂O₂, which then further dissociates into ·OH free radicals. Ultimately, the antibiotic reacts with h... + O2 - The free radicals and ·OH free radicals react and are then decomposed into H2O and CO2.
[0144] Figure 38 The time-resolved fluorescence spectrum of the BiOIO3 photocatalyst powder prepared in Comparative Example 1 is shown, with an excitation wavelength of 340 nm. The decay curves were fitted using a double exponential function, where τ1 corresponds to the photogenerated electrons moving towards oxygen vacancies and Ig. - The relaxation of the induced defect state, τ2 corresponds to the band-band recombination of photogenerated electron-hole pairs. For the BiOIO3 photocatalyst powder prepared in Comparative Example 1, τ1 is 0.7984 ns and τ2 is 4.9672 ns.
[0145] Figure 39 It is the BiO(IO3) prepared in Example 2. 0.96 (VO3) 0.04 Time-resolved fluorescence spectra of the photocatalyst powder were obtained, with an excitation wavelength of 340 nm. Similarly, the decay curves were fitted using a double exponential function, where τ1 corresponds to photogenerated electrons moving to oxygen vacancies and Ig. -The relaxation of induced defect states, τ2 corresponds to band-band recombination of photogenerated electron-hole pairs. For BiO(IO3) 0.96 (VO3) 0.04 Photocatalyst powder, τ1 is 0.9150 ns, τ2 is 7.6193 ns. BiO(IO3) 0.96 (VO3) 0.04 The lifetime of photogenerated carriers in the photocatalyst is longer than that of the BiOIO3 photocatalyst.
[0146] SEM test results show that introducing VO3 into the BiOIO3 lattice... - After the addition of ionic groups, its microstructure changes from irregular nanosheets to nanoribbons, i.e., BiO(IO3). 0.96 (VO3) 0.04 The crystal grows oriented along the
[001] direction, with IO3 / VO3 polar units oriented, resulting in an enhanced macroscopic polarization electric field that promotes the migration of photogenerated carriers from the bulk phase to the surface. Furthermore, VO3... - The introduction of ionic groups and the formation of serrated edges lead to the preparation of BiO(IO3). 0.96 (VO3) 0.04 An increase in the oxygen vacancy concentration in the crystal lattice allows the charge localization effect of oxygen vacancies to promote the migration of photogenerated carriers to active sites on the catalyst surface, thereby suppressing electron-hole recombination. This is achieved by introducing VO3. - Ionic groups on BiO(IO3) 0.96 (VO3) 0.04 By regulating the microstructure, the macroscopic polarization electric field can be enhanced and the oxygen vacancy concentration can be increased, thereby achieving a simultaneous improvement in the bulk phase separation efficiency and surface separation efficiency of photogenerated carriers. This leads to an increase in the separation efficiency and lifetime of photogenerated electron-hole pairs, allowing higher concentrations of photogenerated electrons and holes to participate in photocatalytic reactions.
[0147] Figure 40 The BiO(IO3) prepared in this invention 1-x (VO3) x The EPR spectra of photocatalyst powders under simulated sunlight irradiation for superoxide radicals are shown in the figure. Curves a and c represent the EPR spectra of photocatalyst powders prepared in Comparative Example 1 and Example 2, respectively, under simulated sunlight irradiation for superoxide radicals. In the figure, the four characteristic signal peaks with an intensity ratio of approximately 1:1:1:1 represent the EPR signals of superoxide radicals, indicating that the BiOIO3 photocatalyst prepared in Comparative Example 1 and the BiO(IO3) photocatalyst prepared in Example 2... 0.96 (VO3) 0.04 Photocatalysts can all generate superoxide radicals under simulated sunlight irradiation. The BiO(IO3) prepared in Example 2... 0.96 (VO3) 0.04The EPR signal of the photocatalyst is significantly stronger than that of BiOIO3, indicating that BiO(IO3) has a stronger EPR signal. 0.96 (VO3) 0.04 Under simulated sunlight, a higher concentration of superoxide radicals can be generated to participate in photocatalytic reactions.
[0148] Figure 41 The BiO(IO3) prepared in this invention 1-x (VO3) x The EPR spectra of hydroxyl radicals in the photocatalyst powder under simulated sunlight irradiation are shown in the figure. Curves a and c represent the EPR spectra of hydroxyl radicals in the photocatalyst powders prepared in Comparative Example 1 and Example 2, respectively, under simulated sunlight irradiation. In the figure, the four characteristic signal peaks with an intensity ratio of approximately 1:2:2:1 represent the EPR signals of hydroxyl radicals, indicating that the BiOIO3 photocatalyst prepared in Comparative Example 1 and the BiO(IO3) photocatalyst prepared in Example 2... 0.96 (VO3) 0.04 Photocatalysts can all generate hydroxyl radicals under simulated sunlight irradiation. The BiO(IO3) prepared in Example 2... 0.96 (VO3) 0.04 The EPR signal of the photocatalyst is significantly stronger than that of BiOIO3, indicating that BiO(IO3) has a stronger EPR signal. 0.96 (VO3) 0.04 Under simulated sunlight, a higher concentration of hydroxyl radicals can be generated to participate in photocatalytic reactions.
[0149] Photoelectrochemical testing results, fluorescence spectroscopy, and time-resolved fluorescence spectroscopy results indicate that, compared with the BiO(IO3) photocatalyst, the BiO(IO3) prepared in this invention... 1-x (VO3) x The separation efficiency of photogenerated carriers in the photocatalyst is significantly improved, and the lifetime is extended, and BiO(IO3) 1-x (VO3) x The reduction ability of photogenerated electrons is higher than that of BiOIO3. Therefore, BiO(IO3) 1-x (VO3) x Photocatalysts can generate higher concentrations of superoxide radicals and hydroxyl radicals under simulated sunlight irradiation, which participate in the photocatalytic reaction, resulting in higher photocatalytic performance under simulated sunlight irradiation than pure phase BiOIO3.
[0150] In summary, the BiO(IO3) described in this invention... 1-x (VO3) x The photocatalyst exhibits enhanced visible light absorption and high separation efficiency of photogenerated electron-hole pairs, and demonstrates high degradation activity for antibiotics under ultraviolet light and simulated sunlight irradiation.
Claims
1. BiO(IO3) 1-x (VO3) x A method for preparing a photocatalyst, characterized in that, The photocatalyst has the chemical formula BiO(IO3). 1-x (VO3) x Where x is 0.02-0.06, the photocatalyst exhibits a nanoribbon morphology; the process includes the following steps: Step 1: Disperse Bi(NO3)3•5H2O powder into HNO3 solution and stir to obtain suspension A; Step 2: Under stirring conditions, add KIO3 powder to suspension A and stir to obtain suspension B; Step 3: Under stirring conditions, add NH4VO3 powder to suspension B and stir to obtain reaction precursor solution C; Step 4: Perform a hydrothermal reaction on the precursor solution C; after the reaction is complete, wash and dry the resulting precipitate to obtain BiO(IO3). 1-x (VO3) x Photocatalyst.
2. The BiO(IO3) according to claim 1 1-x (VO3) x A method for preparing a photocatalyst, characterized in that, In the reaction precursor solution C obtained in step 3, the molar ratio of Bi(NO3)3•5H2O to the sum of the molar amounts of KIO3 and NH4VO3 is 1:(1.02-1.06).
3. The BiO(IO3) according to claim 1 1-x (VO3) x A method for preparing a photocatalyst, characterized in that, In the precursor solution C obtained in step 3, the concentrations of Bi(NO3)3•5H2O, HNO3, KIO3, and NH4VO3 were 0.020–0.067 mol·L⁻¹. -1 0.015-0.045 mol·L -1 0.020-0.067 mol·L -1 and 0.0005-0.004 mol·L -1 .
4. The BiO(IO3) according to claim 1 1-x (VO3) x A method for preparing a photocatalyst, characterized in that, In step 4, the hydrothermal reaction temperature is 150-210℃, and the reaction time is 18-32 h.
5. The BiO(IO3) according to claim 1 1-x (VO3) x A method for preparing a photocatalyst, characterized in that, The hydrothermal reactor used in the hydrothermal reaction has a filling ratio of 60%-80%.
6. The BiO(IO3) according to claim 1 1-x (VO3) x A method for preparing a photocatalyst, characterized in that, In step 4, the drying temperature is 50-80℃.
7. The BiO(IO3) according to claim 1 1-x (VO3) x A method for preparing a photocatalyst, characterized in that, With x = 0.04, the photocatalyst exhibits a nanoribbon morphology with serrated edges.
8. BiO(IO3) obtained by the preparation method according to any one of claims 1 to 7. 1-x (VO3) x Photocatalyst.
9. The BiO(IO3) according to claim 8 1-x (VO3) x Application of photocatalysts in the photocatalytic degradation of organic pollutants.
10. The application according to claim 9, characterized in that, The organic pollutant is an antibiotic.
Citation Information
Patent Citations
Preparation method of supported BiOIO3 photo-catalyst
CN104801321A
Tubular carbon nitride-based Schottky heterojunction photocatalyst as well as preparation method and application thereof
CN114984990A