High-temperature-resistant water-based drilling fluid emulsion lubricant and preparation method and application thereof
By preparing a water-based drilling fluid emulsion lubricant containing white oil, oleic acid, polysorbate-80, and surfactant components, the problems of low lubrication performance and insufficient high-temperature resistance of water-based drilling fluids were solved, achieving efficient lubrication in deep wells.
Patent Information
- Application Number
- CN202410344650.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-25
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-03-25
AI Technical Summary
Existing water-based drilling fluids have poor lubrication performance and insufficient high-temperature resistance, making it difficult to meet the drilling and production needs of deep wells and even ultra-deep wells.
A high-temperature resistant water-based drilling fluid emulsion lubricant is prepared by free radical polymerization using a combination of white oil, oleic acid, polysorbate-80, surfactant components and defoamer. The lubricating film of surfactants enhances the film strength and thermal stability of the drill bit surface.
It significantly improves the temperature resistance and stability of the lubricant, enhances the lubrication effect, meets the needs of deep well drilling, reduces frictional resistance, and improves drilling efficiency.
Smart Images

Figure CN118256202B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of drilling fluid lubricants, and more particularly to a high-temperature resistant water-based drilling fluid emulsion lubricant, its preparation method, and its application. Background Technology
[0002] Compared to oil-based drilling fluids, water-based drilling fluids have excellent hydrophilicity, enabling them to absorb and control moisture on the wellbore. They offer high controllability, stability, and environmental friendliness, making them suitable for drilling operations under most geological conditions. Furthermore, water-based drilling fluids are easy to recover and treat after downhole use, making them the most widely used drilling fluid system currently. However, their poor lubrication performance severely restricts their adoption and use in complex well structures such as extended reach wells and horizontal wells. Adding lubricants to water-based drilling fluids can significantly improve the system's lubrication performance, thereby preventing or even reducing or avoiding engineering accidents such as pressure buildup, differential pressure stuck pipe, and drill bit mud buildup.
[0003] Drilling fluid lubricants are diverse, broadly categorized into solid and liquid lubricants. Currently, common solid lubricants for drilling fluids primarily consist of graphite powder and glass microspheres. Solid lubricants can disperse within the mud cake, transforming sliding friction into rolling friction, thereby reducing friction and drag, and preventing mud buildup. However, most existing solid graphite lubricants have limited adsorption capacity on the drill bit surface due to their large particle size, making it difficult to produce a lasting lubrication and drag reduction effect, and potentially leading to drill string clogging, thus affecting their application performance. Furthermore, compared to liquid lubricants, solid lubricants are not as effective at improving drill bit mud buildup. Typical liquid lubricants, on the other hand, usually contain long-chain hydrocarbon structures. Their lubrication mechanism involves the formation of a hydrophobic lubricating film by the long-chain hydrocarbon groups after the lubricant enters the friction surface. This lubricating film improves the wettability of the drill string surface, inhibits the adsorption of drill cuttings and clay particles, prevents frictional contact between drill string components, reduces drilling friction, minimizes drill string mud buildup and stuck pipe problems, and thus improves drill bit drilling efficiency. As drilling depth increases, downhole temperature and pressure rise accordingly. Conventional drilling fluid lubricants, such as alcohol ether lubricants and vegetable oil lubricants, either suffer from conformational changes or even decomposition at high temperatures due to their inherent structural insufficiency, or they are prone to desorption due to weak adsorption to the drill string surface. This leads to decreased lubrication performance, even oil film rupture, and loss of lubrication. In severe cases, it can cause direct friction between the drill string and the casing or wellbore, seriously hindering the development of oil and gas resources in deep and ultra-deep wells. Therefore, drilling fluid lubricants must possess both excellent lubrication performance and excellent temperature resistance to meet the needs of current oil and gas resource development. Overcoming these technical problems and defects has become a key issue that needs to be addressed. Summary of the Invention
[0004] In order to overcome the shortcomings of the prior art, the present invention aims to provide a high-temperature resistant water-based drilling fluid emulsion lubricant, its preparation method and application, which mainly solves the problems of low lubrication performance and low high-temperature resistance in the existing drilling process, making it difficult to meet the needs of deep well and even ultra-deep well drilling and production.
[0005] To achieve the above objectives, the present invention employs the following technical solution:
[0006] In a first aspect, the present invention provides a high-temperature resistant water-based drilling fluid emulsion lubricant, comprising 12%–22% white oil, 5%–15% oleic acid, 5%–12% polysorbate-80, 18%–40% surfactant, 30%–40% water, and 1%–3% defoamer.
[0007] Preferably, the white oil is one of No. 3 white oil, No. 5 white oil, and No. 7 white oil.
[0008] Preferably, the defoamer is one or more of polyether-modified silicone and composite organosilicon.
[0009] Secondly, the present invention provides a method for preparing a high-temperature resistant water-based drilling fluid emulsion lubricant, comprising the following steps:
[0010] S1: Mix white oil, oleic acid, polysorbate-80 and defoamer to obtain the oil phase;
[0011] S2: Mix the surfactant component with water to obtain an aqueous phase;
[0012] S3: Mix the aqueous phase and the oil phase, and after the reaction, obtain the final high-temperature resistant water-based drilling fluid emulsion lubricant.
[0013] Preferably, the reaction conditions in S3 are: a reaction temperature of 40-50°C, a reaction time of 15 min, and a stirring speed of 12000-13000 r / min.
[0014] Preferably, the method for synthesizing the surfactant component is as follows:
[0015] Sodium oleate was dissolved in water to obtain an aqueous solution of sodium oleate; sodium methyl methacrylate was dissolved in water and the pH was adjusted to 8-9. The resulting solution was added to the aqueous solution of sodium oleate; the mixed solution was stirred, heated, and an initiator was added dropwise. After the reaction, the surface-active component was obtained.
[0016] Preferably, the mass concentration of sodium oleate and sodium methacrylate in the surfactant component is 20wt% to 30wt%; and the mass ratio of sodium oleate to sodium methacrylate is 8 to 10:1.
[0017] Preferably, the heating conditions are: reacting at 65-85°C for 6 hours; the stirring conditions are: stirring speed of 1000 r / min.
[0018] Preferably, the initiator is ammonium persulfate; the amount of the initiator is 3% of the total mass of sodium oleate and sodium methyl methacrylate.
[0019] Thirdly, the present invention provides an application of a high-temperature resistant water-based drilling fluid emulsion lubricant in the drilling field.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] This invention prepares an amphiphilic surfactant through free radical polymerization and uses it as an emulsifier in combination with base oils and other substances, enabling the oils to disperse in water in the form of an emulsion, thus fully exerting their lubricating effect in water-based drilling fluids. Furthermore, this surfactant exhibits excellent performance; compared to the method without the addition of surfactant, the high-temperature resistant water-based drilling fluid emulsion lubricant prepared by the method provided in this invention shows significantly enhanced temperature resistance and stability.
[0022] The high-temperature resistant water-based drilling fluid emulsion lubricant of this invention is simple to synthesize, using sodium oleate and sodium methyl methacrylate sulfonate as the main raw materials, which are widely available. The sulfonic acid group contained in the high-temperature resistant water-based drilling fluid emulsion lubricant prepared by this invention is an important metal surface adsorption group. The lubricant modified with polar groups can enhance the film-forming strength between the lubricant and the drill string surface; furthermore, the synergistic effect between the various substances improves the adsorption of lubricant molecules on the metal surface and its thermal stability, thereby producing a better and more durable lubrication effect. Moreover, the selected defoamer product type is sufficient to overcome the foaming problem of emulsion lubricants and meet the performance indicators. Attached Figure Description
[0023] Figure 1 This is a schematic diagram illustrating the preparation process of a high-temperature resistant water-based drilling fluid emulsion lubricant according to the present invention.
[0024] Figure 2 This is a schematic diagram of the preparation process of the surface-active component of the present invention. Detailed Implementation
[0025] To enable those skilled in the art to better understand the present invention, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of the present invention.
[0026] It should be understood that, when used in this specification and the appended claims, the terms "comprising" and "including" indicate the presence of the described features, integrals, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integrals, steps, operations, elements, components and / or collections thereof.
[0027] It should also be understood that the terminology used in this specification is for the purpose of describing particular embodiments only and is not intended to limit the invention. As used in this specification and the appended claims, the singular forms “a,” “an,” and “the” are intended to include the plural forms unless the context clearly indicates otherwise.
[0028] It should also be further understood that the term "and / or" as used in this specification and the appended claims refers to any combination of one or more of the associated listed items and all possible combinations, and includes such combinations.
[0029] The accompanying drawings illustrate various structural schematic diagrams according to embodiments disclosed in this invention. These drawings are not to scale, and some details have been enlarged for clarity, and some details may have been omitted. The shapes of the various regions and layers shown in the drawings, as well as their relative sizes and positional relationships, are merely exemplary and may deviate from reality due to manufacturing tolerances or technical limitations. Furthermore, those skilled in the art can design regions / layers with different shapes, sizes, and relative positions as needed.
[0030] The first objective of this invention is to provide a high-temperature resistant water-based drilling fluid emulsion lubricant, comprising 12%–22% white oil, 5%–15% oleic acid, 5%–12% polysorbate-80, 18%–40% surfactant, 30%–40% water, and 1%–3% defoamer. The white oil is one of No. 3 white oil, No. 5 white oil, or No. 7 white oil.
[0031] Preferably, the high-temperature resistant water-based drilling fluid emulsion lubricant comprises 14-18% white oil, 5-10% oleic acid, 5-10% polysorbate-80, 22-36% surfactant, 34-40% water, and 1.5-3% defoamer.
[0032] More preferably, the high-temperature resistant water-based drilling fluid emulsion lubricant comprises 16% white oil, 7% oleic acid, 6% polysorbate-80, 32% surfactant, 38% water, and 3% defoamer.
[0033] This invention incorporates white oil, which possesses excellent lubricating properties, effectively reducing friction between the drill bit and the wellbore, thus improving drilling efficiency. Secondly, oleic acid is added; as an unsaturated fatty acid, oleic acid has excellent lubricating and rust-preventing properties, protecting the drill bit and wellbore from corrosion and wear. The added polysorbate-80 can uniformly disperse immiscible liquids such as oil and water, forming a stable emulsion, improving the stability and lubrication effect of the drilling fluid. Surfactant components can reduce surface tension, allowing the drilling fluid to more easily penetrate into the tiny gaps between the drill bit and the wellbore, providing a more uniform lubrication effect. Water provides good cooling and cleaning effects, helping to keep the drill bit clean and reduce its temperature, preventing overheating and damage. An antifoaming agent effectively eliminates foam generated during stirring and use of the drilling fluid, ensuring its stability and fluidity, and improving drilling efficiency.
[0034] like Figure 1 As shown, a second objective of this invention is to provide a method for preparing the above-mentioned high-temperature resistant water-based drilling fluid emulsion lubricant, comprising the following steps:
[0035] S1: Mix white oil, oleic acid, polysorbate-80 and defoamer to obtain the oil phase;
[0036] S2: Mix the surfactant component with water to obtain an aqueous phase;
[0037] S3: Mix the aqueous phase and the oil phase, and after the reaction, obtain the final high-temperature resistant water-based drilling fluid emulsion lubricant.
[0038] Preferably, the specific steps of S1 are as follows: white oil, oleic acid, polysorbate-80 and defoamer are mixed, and the mixture is placed in a magnetic stirrer with a stirring speed of 1000 r / min and a temperature of 40-50℃ for 10 min to obtain an oil phase; the reaction conditions in S3 are as follows: reaction temperature of 40-50℃, reaction time of 15 min, and stirring speed of 12000-13000 r / min.
[0039] Among them, such as Figure 2 As shown, the synthesis method of the surface-active component is as follows:
[0040] Sodium oleate was dissolved in water to obtain an aqueous solution of sodium oleate; sodium methyl methacrylate was dissolved in water and the pH was adjusted to 8-9. The resulting solution was added to the aqueous solution of sodium oleate; the mixed solution was stirred, heated, and an initiator was added dropwise. After the reaction, the surface-active component was obtained.
[0041] Preferably, the mass ratio of sodium oleate to sodium methacrylate sulfonate is 8-10:1; the heating conditions are: reaction at 65-85°C for 6 hours; the stirring speed is 1000 r / min; the initiator is ammonium persulfate, and its amount is 3% of the total mass of sodium oleate and sodium methacrylate sulfonate.
[0042] Example 1
[0043] S1: Dissolve 80g of sodium oleate powder in 182.3g of water, filter to remove insoluble impurities, and obtain an aqueous solution of sodium oleate;
[0044] S2: Dissolve 10g of sodium methacrylate in 100g of water to obtain an aqueous solution of sodium methacrylate; add NaOH solution to adjust the pH of the aqueous solution of sodium methacrylate to 8; mix with the aqueous solution of sodium oleate, add the mixed solution to a three-necked flask, insert a thermometer, place a magnetic stir bar, set the magnetic stirring speed to 1000r / min, reflux, heat to 75℃, start timing, and start adding 2.7g of initiator ammonium persulfate. React for 6h, and finally cool to room temperature to obtain the surface active component;
[0045] S3: Mix 14g of No. 5 white oil, 7g of oleic acid, 8g of polysorbate-80 and 3g of composite organosilicon defoamer, place in a magnetic stirrer, stir at 1000r / min, control the temperature at 42℃, stir for 10min, and the first mixture is obtained after mixing, which is recorded as the oil phase;
[0046] S4: Mix 20g of surfactant component and 38g of water, heat to 42℃ to obtain a second mixture, denoted as the aqueous phase;
[0047] S5: After the oil and water phases stop heating, immediately add the water phase dropwise into the oil phase, and complete the water phase dropwise addition within 5 minutes; and emulsify under the action of a homogenizer, and homogenize and emulsify for 15 minutes (excluding the water phase dropwise addition time) at a stirring speed of 12500 r / min. The water-based drilling fluid emulsion lubricant is obtained after the emulsification is completed.
[0048] Example 2
[0049] S1: Dissolve 80g of sodium oleate powder in 182.3g of water, filter to remove insoluble impurities, and obtain an aqueous solution of sodium oleate;
[0050] S2: Dissolve 10g of sodium methacrylate in 100g of water to obtain an aqueous solution of sodium methacrylate; add NaOH solution to adjust the pH of the aqueous solution of sodium methacrylate to 8; mix with the aqueous solution of sodium oleate, add the mixed solution to a three-necked flask, insert a thermometer, place a magnetic stir bar, set the magnetic stirring speed to 1000r / min, reflux, heat to 75℃, start timing, and start adding 2.7g of initiator ammonium persulfate. React for 6h, and finally cool to room temperature to obtain the surface active component;
[0051] S3: Mix 16g of No. 5 white oil, 10g of oleic acid, 10g of polysorbate-80 and 3g of composite organosilicon defoamer, place them in a magnetic stirrer, stir at 1000r / min, control the temperature at 42℃, stir for 10min, and the first mixture is obtained after mixing, which is recorded as the oil phase;
[0052] S4: Mix 22g of surfactant component and 36g of water, heat to 42℃ to obtain a second mixture, denoted as the aqueous phase;
[0053] S5: After the oil and water phases stop heating, immediately add the water phase dropwise into the oil phase, and complete the water phase dropwise addition within 5 minutes; and emulsify under the action of a homogenizer, and homogenize and emulsify for 15 minutes (excluding the water phase dropwise addition time) at a stirring speed of 12500 r / min. The water-based drilling fluid emulsion lubricant is obtained after the emulsification is completed.
[0054] Example 3
[0055] S1: Dissolve 80g of sodium oleate powder in 182.3g of water, filter to remove insoluble impurities, and obtain an aqueous solution of sodium oleate;
[0056] S2: Dissolve 10g of sodium methacrylate in 100g of water to obtain an aqueous solution of sodium methacrylate; add NaOH solution to adjust the pH of the aqueous solution of sodium methacrylate to 8; mix with the aqueous solution of sodium oleate, add the mixed solution to a three-necked flask, insert a thermometer, place a magnetic stir bar, set the magnetic stirring speed to 1000r / min, reflux, heat to 75℃, start timing, and start adding 2.7g of initiator ammonium persulfate. React for 6h, and finally cool to room temperature to obtain the surface active component;
[0057] S3: Mix 16g of No. 5 white oil, 7g of oleic acid, 6g of polysorbate-80 and 3g of composite organosilicon defoamer, place them in a magnetic stirrer, stir at 1000r / min, control the temperature at 42℃, stir for 10min, and the first mixture is obtained after mixing, which is recorded as the oil phase;
[0058] S4: Mix 32g of surfactant component and 38g of water, heat to 42℃ to obtain a second mixture, denoted as the aqueous phase;
[0059] S5: After the oil and water phases stop heating, immediately add the water phase dropwise into the oil phase, and complete the water phase dropwise addition within 5 minutes; and emulsify under the action of a homogenizer, and homogenize and emulsify for 15 minutes (excluding the water phase dropwise addition time) at a stirring speed of 12500 r / min. The water-based drilling fluid emulsion lubricant is obtained after the emulsification is completed.
[0060] Example 4
[0061] S1: Dissolve 80g of sodium oleate powder in 182.3g of water, filter to remove insoluble impurities, and obtain an aqueous solution of sodium oleate;
[0062] S2: Dissolve 10g of sodium methacrylate in 100g of water to obtain an aqueous solution of sodium methacrylate; add NaOH solution to adjust the pH of the aqueous solution of sodium methacrylate to 8; mix with the aqueous solution of sodium oleate, add the mixed solution to a three-necked flask, insert a thermometer, place a magnetic stir bar, set the magnetic stirring speed to 1000r / min, reflux, heat to 75℃, start timing, and start adding 2.7g of initiator ammonium persulfate. React for 6h, and finally cool to room temperature to obtain the surface active component;
[0063] S3: Mix 18g of No. 5 white oil, 7g of oleic acid, 14g of polysorbate-80 and 3g of composite organosilicon defoamer, place them in a magnetic stirrer, stir at 1000r / min, control the temperature at 42℃, stir for 10min, and the first mixture is obtained after mixing, which is recorded as the oil phase;
[0064] S4: Mix 22g of surfactant component and 32g of water, heat to 42℃ to obtain a second mixture, denoted as the aqueous phase;
[0065] S5: After the oil and water phases stop heating, immediately add the water phase dropwise into the oil phase, and complete the water phase dropwise addition within 5 minutes; and emulsify under the action of a homogenizer, and homogenize and emulsify for 15 minutes (excluding the water phase dropwise addition time) at a stirring speed of 12500 r / min. The water-based drilling fluid emulsion lubricant is obtained after the emulsification is completed.
[0066] Example 5
[0067] S1: Dissolve 80g of sodium oleate powder in 182.3g of water, filter to remove insoluble impurities, and obtain an aqueous solution of sodium oleate;
[0068] S2: Dissolve 10g of sodium methacrylate in 100g of water to obtain an aqueous solution of sodium methacrylate; add NaOH solution to adjust the pH of the aqueous solution of sodium methacrylate to 8; mix with the aqueous solution of sodium oleate, add the mixed solution to a three-necked flask, insert a thermometer, place a magnetic stir bar, set the magnetic stirring speed to 1000r / min, reflux, heat to 75℃, start timing, and start adding 2.7g of initiator ammonium persulfate. React for 6h, and finally cool to room temperature to obtain the surface active component;
[0069] S3: Mix 18g of No. 5 white oil, 10g of oleic acid, 8g of polysorbate-80 and 3g of composite organosilicon defoamer, place in a magnetic stirrer, stir at 1000r / min, control the temperature at 42℃, stir for 10min, and the first mixture is obtained after mixing, which is recorded as the oil phase;
[0070] S4: Mix 18g of surfactant component and 40g of water, heat to 42℃ to obtain a second mixture, denoted as the aqueous phase;
[0071] S5: After the oil and water phases stop heating, immediately add the water phase dropwise into the oil phase, and complete the water phase dropwise addition within 5 minutes; and emulsify under the action of a homogenizer, and homogenize and emulsify for 15 minutes (excluding the water phase dropwise addition time) at a stirring speed of 12500 r / min. The water-based drilling fluid emulsion lubricant is obtained after the emulsification is completed.
[0072] Example 6
[0073] S1: Dissolve 80g of sodium oleate powder in 182.3g of water, filter to remove insoluble impurities, and obtain an aqueous solution of sodium oleate;
[0074] S2: Dissolve 10g of sodium methacrylate in 100g of water to obtain an aqueous solution of sodium methacrylate; add NaOH solution to adjust the pH of the aqueous solution of sodium methacrylate to 8; mix with the aqueous solution of sodium oleate, add the mixed solution to a three-necked flask, insert a thermometer, place a magnetic stir bar, set the magnetic stirring speed to 1000r / min, reflux, heat to 75℃, start timing, and start adding 2.7g of initiator ammonium persulfate. React for 6h, and finally cool to room temperature to obtain the surface active component;
[0075] S3: Mix 20g of No. 5 white oil, 10g of oleic acid, 12g of polysorbate-80 and 3g of composite organosilicon defoamer, place them in a magnetic stirrer, stir at 1000r / min, control the temperature at 42℃, stir for 10min, and the first mixture is obtained after mixing, which is recorded as the oil phase;
[0076] S4: Mix 24g of surfactant component and 34g of water, heat to 42℃ to obtain a second mixture, denoted as the aqueous phase;
[0077] S5: After the oil and water phases stop heating, immediately add the water phase dropwise into the oil phase, and complete the water phase dropwise addition within 5 minutes; and emulsify under the action of a homogenizer, and homogenize and emulsify for 15 minutes (excluding the water phase dropwise addition time) at a stirring speed of 12500 r / min. The water-based drilling fluid emulsion lubricant is obtained after the emulsification is completed.
[0078] Example 7
[0079] S1: Dissolve 80g of sodium oleate powder in 257.3g of water, filter to remove insoluble impurities, and obtain an aqueous solution of sodium oleate;
[0080] S2: Dissolve 10g of sodium methacrylate in 100g of water to obtain an aqueous solution of sodium methacrylate; adjust the pH of the aqueous solution of sodium methacrylate to 8.5 by adding NaOH solution; mix with the aqueous solution of sodium oleate, add the mixed solution to a three-necked flask, insert a thermometer, place a magnetic stir bar, set the magnetic stirring speed to 1000r / min, reflux, heat to 85℃, start timing, and start adding 2.7g of initiator ammonium persulfate. React for 3h, and finally cool to room temperature to obtain the surface active component.
[0081] S3: Mix 12g of No. 3 white oil, 12g of oleic acid, 5g of polysorbate-80 and 1g of polyether modified silicone defoamer, place them in a magnetic stirrer, stir at 1000r / min, control the temperature at 40℃, stir for 10min, and the first mixture is obtained after mixing, which is called the oil phase;
[0082] S4: Mix 40g of surfactant component and 30g of water, heat to 40℃ to obtain a second mixture, denoted as the aqueous phase;
[0083] S5: After the oil and water phases stop heating, immediately add the water phase dropwise into the oil phase, and complete the water phase dropwise addition within 5 minutes; and emulsify under the action of a homogenizer, and homogenize and emulsify for 15 minutes (excluding the water phase dropwise addition time) at a stirring speed of 12000 r / min. The water-based drilling fluid emulsion lubricant is obtained after the emulsification is completed.
[0084] Example 8
[0085] S1: Dissolve 100g of sodium oleate powder in 226.7g of water, filter to remove insoluble impurities, and obtain an aqueous solution of sodium oleate;
[0086] S2: Dissolve 10g of sodium methacrylate in 100g of water to obtain an aqueous solution of sodium methacrylate; add NaOH solution to adjust the pH of the aqueous solution of sodium methacrylate to 9; mix with the aqueous solution of sodium oleate, add the mixed solution to a three-necked flask, insert a thermometer, place a magnetic stir bar, set the magnetic stirring speed to 1000r / min, reflux, heat to 65℃, start timing, and start adding 3.3g of ammonium persulfate as initiator. React for 6h, and finally cool to room temperature to obtain the surface active component;
[0087] S3: Mix 22g of No. 3 white oil, 5g of oleic acid, 11g of polysorbate-80 and 2g of polyether modified silicone defoamer, place them in a magnetic stirrer, stir at 1000r / min, control the temperature at 48℃, stir for 10min, and the first mixture is obtained after mixing, which is recorded as the oil phase;
[0088] S4: Mix 30g of surfactant component and 30g of water, heat to 48℃ to obtain a second mixture, denoted as the aqueous phase;
[0089] S5: After the oil and water phases stop heating, immediately add the water phase dropwise into the oil phase, and complete the water phase dropwise addition within 5 minutes; and emulsify under the action of a homogenizer, and homogenize and emulsify for 15 minutes (excluding the water phase dropwise addition time) at a stirring speed of 12800 r / min. The water-based drilling fluid emulsion lubricant is obtained after the emulsification is completed.
[0090] Example 9
[0091] S1: Dissolve 80g of sodium oleate powder in 167.3g of water, filter to remove insoluble impurities, and obtain an aqueous solution of sodium oleate;
[0092] S2: Dissolve 10g of sodium methacrylate in 100g of water to obtain an aqueous solution of sodium methacrylate; add NaOH solution to adjust the pH of the aqueous solution of sodium methacrylate to 9; mix with the aqueous solution of sodium oleate, add the mixed solution to a three-necked flask, insert a thermometer, place a magnetic stir bar, set the magnetic stirring speed to 1000r / min, reflux, heat to 80℃, start timing, and start adding 2.7g of initiator ammonium persulfate. React for 5h, and finally cool to room temperature to obtain the surface active component.
[0093] S3: Mix 15g of No. 7 white oil, 15g of oleic acid, 10g of polysorbate-80 and 1.5g of polyether modified silicone type and composite organosilicon type mixed defoamer, place them in a magnetic stirrer, stir at a speed of 1000r / min, control the temperature at 50℃, stir for 10min, and the first mixture is obtained after mixing, which is recorded as the oil phase;
[0094] S4: Mix 28g of surfactant component and 30g of water, heat to 50℃ to obtain a second mixture, denoted as the aqueous phase;
[0095] S5: After the oil and water phases stop heating, immediately add the water phase dropwise into the oil phase, and complete the water phase dropwise addition within 5 minutes; and emulsify under the action of a homogenizer, and homogenize and emulsify for 15 minutes (excluding the water phase dropwise addition time) at a stirring speed of 13000 r / min. The water-based drilling fluid emulsion lubricant is obtained after the emulsification is completed.
[0096] Comparative Example
[0097] S1: Dissolve 80g of sodium oleate powder in 182.3g of water, filter to remove insoluble impurities, and obtain an aqueous solution of sodium oleate;
[0098] S2: Dissolve 10g of sodium methacrylate in 100g of water to obtain an aqueous solution of sodium methacrylate; add NaOH solution to adjust the pH of the aqueous solution of sodium methacrylate to 8; mix with the aqueous solution of sodium oleate, add the mixed solution to a three-necked flask, insert a thermometer, place a magnetic stir bar, set the magnetic stirring speed to 1000r / min, reflux, heat to 75℃, start timing, and start adding 2.7g of initiator ammonium persulfate. React for 6h, and finally cool to room temperature to obtain the surface active component;
[0099] S3: Mix 16g of No. 5 white oil, 6g of polysorbate-80 and 3g of composite silicone defoamer, place in a magnetic stirrer, stir at 1000r / min, control the temperature at 42℃, stir for 10min, and the first mixture is obtained after mixing, which is recorded as the oil phase;
[0100] S4: Mix 32g of surfactant component and 38g of water, heat to 42℃ to obtain a second mixture, denoted as the aqueous phase;
[0101] S5: After the oil and water phases stop heating, immediately add the water phase dropwise into the oil phase, and complete the water phase dropwise addition within 5 minutes; and emulsify under the action of a homogenizer, and homogenize and emulsify for 15 minutes (excluding the water phase dropwise addition time) at a stirring speed of 12500 r / min. The water-based drilling fluid emulsion lubricant is obtained after the emulsification is completed.
[0102] Performance testing
[0103] The performance result testing method in this invention is as follows:
[0104] (1) Preparation of base slurry: Prepare the base slurry according to the ratio of calcium-based bentonite: anhydrous sodium carbonate: distilled water = 25g: 1g: 500mL. Stir the base slurry for 60min at 10000r / min using a high-speed mixer GJSS-B12K and cure it in a sealed container at room temperature for 24h to obtain the base slurry.
[0105] (2) Preparation of 4% brine base slurry: Take 300mL of aged base slurry, add 12g NaCl to it, stir with a high-speed mixer GJSS-B12K at 10000r / min speed for 20min, and seal for 24h for later use.
[0106] (3) Preparation of saturated brine base slurry: Take 300 mL of aged base slurry, add 108 g NaCl to it, stir with a high-speed mixer GJSS-B12K at 10000 r / min for 20 min, and seal for 24 h for later use.
[0107] (4) Determination of foaming rate: Take 300 mL of aged base slurry, add 0.5% lubricant sample, and stir with a high-speed mixer GJSS-B12K at 11000 r / min for 5 min. Start timing after stirring stops, pour the slurry into a 500 mL graduated cylinder within 20 s, read the volume within 30 s, and calculate the foaming rate using the following formula:
[0108]
[0109] Where: p—foaming rate, %; V—volume of 300mL base slurry after high stirring, mL.
[0110] (5) Lubrication coefficient reduction rate determination: Take 300 mL of aged base slurry, add 0.5% lubricant sample, and stir with a high-speed mixer at 11000 r / min for 5 min. Test using a digital display EP-extreme pressure lubrication instrument: turn on the motor, control it at 60 RPM and 150 inch-pound torque, run for 5 min, and determine the lubrication coefficient of the base slurry and the lubrication coefficient after adding the sample. The test conditions for the base slurry and the lubrication coefficient after adding the sample should be completely consistent.
[0111] Calculate the lubrication coefficient reduction rate using the following formula:
[0112]
[0113] Where: R—reduction rate of lubrication coefficient, %; K0—lubrication coefficient of base slurry; K1—lubrication coefficient of sample slurry.
[0114] According to the technical requirements specified in Q / SY17088-2016 "Technical Specification for Liquid Lubricants for Drilling Fluids", the performance of drilling fluids after adding the water-based drilling fluid emulsion lubricants obtained in Examples 1-6 and comparative examples of this invention was measured, and the results are shown in Table 1:
[0115] Table 1. Performance of drilling fluids after adding lubricants obtained in Examples 1-6 and comparative examples.
[0116]
[0117]
[0118] As can be seen from the data in Table 1, the lubrication coefficient reduction rate of the drilling fluids with added lubricants from Examples 1 to 6 of the present invention is greater than 84%, which is better than the specified standard of ≥80%, and the foaming rate is ≤10%. Therefore, it can be seen that the lubricants from Examples 1 to 6 of the present invention have excellent lubrication performance.
[0119] High-temperature resistance test: The lubricity of the drilling fluid after adding the lubricant obtained in Example 3 of this invention was tested after aging at room temperature (120-180℃) for 16 hours. The results are shown in Table 2.
[0120] Table 2 shows the lubricity of the drilling fluid after adding the lubricant obtained in Example 3.
[0121]
[0122] As can be seen from the data in Table 2, when the aging temperature of the drilling fluid containing the lubricant of Example 3 of the present invention is raised to 180°C, the lubrication coefficient reduction rate can still be maintained at more than 76%; this shows that the lubricant of Example 3 of the present invention has excellent high temperature resistance.
[0123] Therefore, the raw materials for the lubricant of the present invention are readily available, the synthesis process is relatively simple, it has strong water dispersibility and stable structure, and it exhibits excellent lubrication and temperature resistance in bentonite drilling fluid-based slurries, thus showing potential for application in drilling fluid lubrication.
[0124] The above content is only for illustrating the technical concept of the present invention and should not be construed as limiting the scope of protection of the present invention. Any modifications made to the technical solution based on the technical concept proposed in this invention shall fall within the scope of protection of the claims of this invention.
Claims
1. A high temperature resistant water-based drilling fluid emulsion lubricant characterized by, The high-temperature-resistant water-based drilling fluid emulsion lubricant comprises white oil 12%-22%, oleic acid 5%-15%, polysorbate-80 5%-12%, a surface active component 18%-40%, water 30%-40%, and an antifoaming agent 1%-3%. The synthesis method of the surface active component is as follows: Dissolving sodium oleate in water to obtain a sodium oleate aqueous solution; dissolving sodium methallyl sulfonate in water and adjusting the pH to 8-9, and then adding the obtained solution into the sodium oleate aqueous solution; stirring, heating, and dropwise adding an initiator to the mixed solution, and then obtaining the surface active component after reaction; The mass concentration of sodium oleate and sodium methallyl sulfonate in the surface active component is 20wt%-30wt%, and the mass ratio of sodium oleate to sodium methallyl sulfonate is (8-10):
1. The initiator is ammonium persulfate, and the amount of the initiator is 3% of the total mass of sodium oleate and sodium methallyl sulfonate.
2. A high temperature resistant water-based drilling fluid emulsion lubricant as claimed in claim 1, wherein, The white oil is one of No. 3 white oil, No. 5 white oil, and No. 7 white oil.
3. A high temperature resistant water based drilling fluid emulsion lubricant as claimed in claim 1 wherein, The antifoaming agent is one or more of polyether-modified silicon type and composite silicone type.
4. A high temperature resistant water-based drilling fluid emulsion lubricant as defined in claim 1, wherein, The heating condition is that the reaction is carried out at 65-85℃ for 6h, and the stirring condition is that the stirring speed is 1000r / min.
5. A method of preparing a high temperature resistant water-based drilling fluid emulsion lubricant as claimed in any one of claims 1 to 4, characterized in that, The method comprises the following steps: S1: mixing white oil, oleic acid, polysorbate-80, and an antifoaming agent to obtain an oil phase; S2: mixing a surface active component and water to obtain an aqueous phase; S3: mixing the aqueous phase and the oil phase, and then obtaining the final high-temperature-resistant water-based drilling fluid emulsion lubricant after reaction.
6. A method of preparing a high temperature resistant water based drilling fluid emulsion lubricant as claimed in claim 5, wherein, The reaction condition in S3 is that the reaction temperature is 40-50℃, the reaction time is 15min, and the stirring speed is 12000-13000r / min.
7. Application of the high-temperature-resistant water-based drilling fluid emulsion lubricant according to any one of claims 1-4 in the field of drilling.
Citation Information
Patent Citations
Nano lubricant for drilling fluid as well as preparation method and application of nano lubricant
CN113265023A
High-temperature-resistant quick drilling agent, preparation method thereof and application of high-temperature-resistant quick drilling agent in water-based drilling fluid
CN115197679A