A method of enhancing a flue gas circulating sintering

By adding bentonite to the sintering batch and adjusting the flue gas circulation method, the problem of insufficient oxygen content in the flue gas was solved, the quality of sintered ore and fuel combustion efficiency were improved, and the wind-oxygen balance was improved, as well as the environmental protection and energy-saving effects were achieved.

CN118256711BActive Publication Date: 2026-11-24武汉钢铁有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410375407.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-29
Publication Date
2026-11-24
Estimated Expiration
2044-03-29

AI Technical Summary

Technical Problem

In existing flue gas recirculation processes, insufficient oxygen content in the flue gas leads to a decline in the quality of sintered ore, an increase in wind resistance, and affects the oxidizing atmosphere and fuel combustion efficiency during the sintering process, failing to meet the air volume and oxygen balance requirements of the sintering process.

Method used

Bentonite is added during the sintering process, and the flue gas circulation mode is adjusted so that flue gas at different temperatures is mixed and circulated to different parts of the sintering machine. The flue gas is circulated to the front and rear parts of the sintering machine through the flue gas hood to improve the air volume and oxygen supply to the material surface.

Benefits of technology

It effectively improves the air-oxygen balance in the flue gas recirculation sintering process, enhances the quality of sintered ore, reduces CO emissions, and lowers solid fuel consumption, resulting in significant economic and environmental benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004766905290000011
    Figure HDA0004766905290000011
Patent Text Reader

Abstract

This invention discloses a method for enhancing flue gas recirculation sintering, including batching, granulation, material distribution, and flue gas recirculation sintering steps. The main steps include: 1) In the batching process, bentonite, iron ore, flux, and fuel are used as the main raw materials, mixed, and granulated to obtain a mixed sintering material; 2) Flue gas recirculation sintering; the sintering machine is divided into front and rear sections along the trolley's running direction, and the sintering flue gas is divided into head flue gas, middle flue gas, and tail flue gas along the sintering machine's running direction; the tail flue gas in the sintering flue gas is mixed with the hot exhaust gas from the sintering ring cooler and circulated to the front section of the sintering machine through a flue gas hood; the head flue gas and middle flue gas in the sintering flue gas are mixed and circulated to the rear section of the sintering machine through a flue gas hood. The method described in this invention can effectively improve the oxygen content of the recirculated flue gas and ensure the quality of the sintered ore product. Furthermore, the involved processes are simple, easy to operate, and have good economic and environmental benefits, making it suitable for widespread application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of iron and steel metallurgy technology, and specifically relates to a method for enhancing flue gas circulation sintering. Background Technology

[0002] Against the backdrop of energy conservation and emission reduction in the steel industry, flue gas recirculation technology has gradually become a research hotspot for the green and low-carbon development of sintering. Sintering flue gas recirculation is a method that selectively returns a portion of the heat-carrying flue gas generated during sintering, after certain pretreatment, to the flue gas sealing hood on the upper part of the sintering machine trolley for recycling. The main purpose of sintering flue gas recirculation technology is to recover waste heat and latent heat from the sintering flue gas, reduce the combustion consumption of sintered solids, reduce carbon emissions during the sintering process, and reduce the amount of waste gas to be treated by the desulfurization and denitrification systems. Studies have found that sintering flue gas recirculation technology can reduce flue gas emissions by 25-40%, while also significantly improving dust and SO2 control. x Removal rate, reducing NO x And the amount of dioxins produced.

[0003] Currently, there are five typical flue gas recirculation (FGR) processes: Bao-Steel Flue Gas Recirculation, Nippon Steel's regional FGR process, EOS, LEEP, and EPOSINT. Studies have shown that when the FGR process reaches a recirculation rate of 50%, the O2 volume fraction in the flue gas is only 11.6%; when the LEEP process reaches a recirculation rate of 47%, the O2 volume fraction is only 16%; and when the EPOSINT process reaches a recirculation rate of 23%, the O2 volume fraction is only 13.5%. Problems with existing FGR processes include: 1. Airflow and oxygen balance control in the FGR process: Sintering circulating flue gas is characterized by high temperature, low oxygen, and high moisture content. When using a FGR process, the operating volume of the high-temperature flue gas will be significantly higher than the standard volume, resulting in a substantial increase in air resistance. When the flue gas recirculation ratio is high, the oxygen content of the air entering the sintering bed cannot meet the requirements of the sintering process, leading to incomplete fuel combustion, a weakened oxidizing atmosphere, and hindered formation of acicular calcium ferrite, thus restricting the improvement of sinter quality. Insufficient flue gas oxygen content will reduce sinter productivity by more than 10% and drum strength by more than 12%. 2. When the flue gas recirculation ratio is high, the oxygen content of the air entering the sintering bed cannot meet the requirements of the sintering process, leading to incomplete fuel combustion, a weakened oxidizing atmosphere, and hindered formation of acicular calcium ferrite, severely affecting sinter quality. Insufficient flue gas oxygen content will reduce sinter productivity by more than 10%, drum strength by more than 12%, and calcium ferrite content in the sinter by more than 3%.

[0004] Current research focuses on strengthening the control of oxygen balance in flue gas recirculation processes, primarily addressing the issue of low oxygen volume fraction in the recirculating flue gas. This mainly includes: 1. introducing pure oxygen into the recirculating flue gas; and 2. reducing the temperature of the recirculating flue gas. However, the first method significantly increases sintering costs due to the high price of pure oxygen; the second method, reducing the temperature of the recirculating flue gas, cannot effectively realize the energy-saving and emission-reduction benefits of flue gas recirculation sintering. Summary of the Invention

[0005] The main objective of this invention is to address the problems and shortcomings of existing sintering flue gas recirculation technology, such as the limitation of flue gas oxygen content, the inability of flue gas recirculation air volume and oxygen balance to meet the needs of the sintering process, and the resulting serious deterioration of sintered mineral quality indicators. This invention provides a method for enhancing flue gas recirculation sintering, which effectively improves the adverse effects of insufficient flue gas oxygen content on the quality of sintered products.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0007] A method for enhancing flue gas recirculation sintering includes the steps of batching, granulation, material distribution, and flue gas recirculation sintering, wherein:

[0008] 1) During the batching process, bentonite, iron ore, flux, and fuel are used as the main raw materials and mixed to obtain a mixed sintering material;

[0009] 2) After granulation, the sintering mixture is distributed on the sintering machine trolley for flue gas circulation sintering. Specific steps include: dividing the sintering machine into front and rear sections along the trolley's running direction; the front section extends from the ignition point to 1 / 3 to 2 / 3 of the sintering machine's length; the sintering flue gas is divided into head flue gas, middle flue gas, and tail flue gas along the sintering machine's running direction; the head flue gas is collected from the bellows located from the ignition point to 1 / 10 to 1 / 5 of the sintering machine's length (along the sintering flue gas running direction); the tail flue gas is collected from the bellows located from the tail of the sintering machine (opposite to the sintering flue gas running direction) to 1 / 10 to 1 / 5 of the sintering machine's length; the middle flue gas is collected from the bellows located between the head and tail flue gas sections.

[0010] In the flue gas recirculation step, the tail flue gas with higher temperature in the sintering flue gas is mixed with the hot exhaust gas from the sintering ring cooler and circulated to the front part of the sintering machine through the flue gas hood; the head flue gas with lower temperature in the sintering flue gas is mixed with the middle flue gas and circulated to the rear part of the sintering machine through the flue gas hood.

[0011] In the above scheme, the bentonite accounts for 0.1% to 1.0% of the total mass of the mixed sinter.

[0012] In the above scheme, the main chemical components and their mass percentages in the mixed sintering material include: TFe 55-60%, CaO 8.0-11.0%, and SiO2 4.8-6.0%.

[0013] In the above scheme, the flux can be one or more of dolomite, limestone, quicklime, etc.

[0014] In the above scheme, the fuel can be one or more of coke powder, anthracite, etc., and its content accounts for 3.5 to 4.5% of the total mass of the mixed sinter.

[0015] In the above scheme, the iron ore accounts for 55-65% of the total mass of the mixed sinter.

[0016] Furthermore, in step 1), recycled ore is further introduced during the batching process, accounting for 20-25% of the total mass of the mixed sinter.

[0017] In the above scheme, the average particle size of the sintered mixture obtained by the granulation step is 3-4 mm.

[0018] In the above scheme, during the fabric application process, the thickness of the material layer is controlled to be above 800mm.

[0019] In the above scheme, the process parameters adopted in the flue gas circulation sintering step include: ignition temperature 900~1100℃, ignition time 5~8min, ignition negative pressure 6~8kPa; sintering negative pressure constant 12~13kPa; cooling negative pressure 6~8kPa.

[0020] In the above scheme, the tail gas with a higher temperature in the sintering flue gas is mixed with the hot exhaust gas from the sintering ring cooler, and the temperature of the flue gas after mixing is 200-450℃.

[0021] In the above scheme, the head flue gas and the middle flue gas with lower temperature in the sintering flue gas are mixed, and the temperature of the flue gas after mixing is 100-150℃.

[0022] From a practical production perspective, oxygen balance control in flue gas recirculation is a crucial aspect of the sintering flue gas recirculation process. The effective oxygen content in the sintering inlet air is positively correlated with the effective airflow over the material surface and the oxygen volume fraction in the circulating flue gas; therefore, increasing the airflow over the material surface is an effective way to increase the oxygen content in the sintering inlet air. According to the Voice formula Q=P·F(ΔP·h) -1 ) n (In the formula: Q - air volume through the material layer, P - air permeability index, F - exhaust area, ΔP - exhaust negative pressure, h - material layer height), the air volume through the material layer is positively correlated with the air permeability index of the material layer.

[0023] To address the problem of insufficient oxygen content during sintering caused by flue gas recirculation, this invention provides a method for enhancing flue gas recirculation sintering. Bentonite is incorporated into the sintering batching process, and the flue gas recirculation method is adjusted accordingly. The higher-temperature tail flue gas from the sintering process is mixed with the hot exhaust gas from the sintering ring cooler and circulated to the front of the sintering machine through a flue gas hood. The lower-temperature head flue gas from the sintering process is mixed with the middle flue gas and circulated to the rear of the sintering machine through a flue gas hood.

[0024] Bentonite enhances the granulation performance of sintering raw materials, improves the average particle size and strength of granulated pellets in the mixture, reduces the adhesion between granulated pellets in the wet zone, and improves the cold and hot permeability of the mixture layer. Under conditions of high circulating flue gas volume, it increases the effective airflow through the material surface. Based on the influence of bentonite on the circulating sintering airflow, this invention simultaneously adjusts the sintering flue gas circulation method. The higher-temperature tail flue gas and the hot exhaust gas from the sintering ring cooler are mixed and circulated to the front of the sintering machine through a flue gas hood; the lower-temperature head flue gas and the middle flue gas are mixed and circulated to the rear of the sintering machine through a flue gas hood. During flue gas circulating sintering, due to the significant increase in the effective airflow through the material surface, the sintering speed at the top of the material layer accelerates, and the high-temperature holding time is shortened. Therefore, circulating the higher-temperature flue gas to the front of the sintering machine extends the high-temperature time, allowing for more complete calcium ferrite crystallization. When sintering reaches the lower part of the material layer, due to material segregation, the fuel particles in the lower part are larger and the combustion zone becomes wider. Therefore, the lower temperature flue gas is circulated to the rear end of the sintering machine to improve heat transfer efficiency and accelerate the sintering speed.

[0025] This invention combines ingredient optimization (incorporation of bentonite) with improved flue gas recirculation methods, which can effectively increase the air volume and oxygen supply during the sintering process and enhance the quality indicators of sintered minerals under flue gas recirculation conditions.

[0026] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0027] (1) This invention addresses the problem of difficulty in controlling the oxygen balance in flue gas circulating sintering. Bentonite is added during the sintering batching process to improve the average particle size of the sintering raw materials. Under the condition of relatively insufficient oxygen content in the circulating flue gas, the oxygen content of the flue gas circulating sintering and the oxygen consumption in the sintering process are balanced by increasing the air volume on the material surface. This can effectively improve the problem of insufficient oxygen content in the circulating flue gas, which leads to serious deterioration of the quality of sintered minerals. This is of great significance for achieving clean and energy-saving practices in the iron and steel metallurgical industry.

[0028] (2) Based on the addition of bentonite to the raw materials for flue gas circulation sintering, this invention divides the sintering flue gas into tail flue gas with higher temperature, hot exhaust gas from the sintering ring cooler, and head flue gas and middle flue gas with lower temperature. By adjusting the circulation of flue gas at different temperatures to different parts of the sintering machine, the sintering flue gas can be rationally utilized. Only a small amount of equipment and facilities are added to the existing process. It is low-cost and easy to operate, and is suitable for promotion and application.

[0029] (3) The enhanced flue gas circulation sintering method of the present invention can increase the air intake of the flue gas circulation sintering material surface, enhance the oxidizing atmosphere in the sintering process, reduce CO emissions in the sintering process, improve fuel combustion efficiency in the sintering process, and reduce solid fuel consumption in the sintering process, which has significant economic and environmental benefits. Attached Figure Description

[0030] Figure 1 This is a schematic flowchart of an embodiment of the enhanced flue gas circulation sintering method of the present invention;

[0031] In the diagram, 1 corresponds to the mixed flue gas at the tail end of the wind box and the exhaust gas from the sintering ring cooler; 2 corresponds to the mixed flue gas at the head and middle of the wind box; 3 is the mixed material layer with added bentonite; 4 is the flue gas at the tail end of the sintering machine wind box; 5 is the flue gas in the middle of the sintering machine wind box; and 6 is the flue gas at the head of the sintering machine wind box. Detailed Implementation

[0032] To further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. These descriptions are only for further illustrating the features and advantages of the present invention, and are not intended to limit the scope of the claims of the present invention.

[0033] In the following examples, the main chemical components and their mass percentages in the blended iron ore are: TFe 60.34%, CaO 0.42%, and SiO2 4.79%; the main chemical components and their mass percentages in the return ore are: TFe 55.02%, CaO 9.24%, and SiO2 6.12%.

[0034] The sintering machine used has an area of ​​660m². 2 30 bellows are set on the left and right sides along the direction of operation.

[0035] The sintering parameters used are as follows: ignition temperature 900℃, ignition time 5min, ignition negative pressure 6kPa; constant sintering negative pressure 12kPa; cooling negative pressure 6kPa.

[0036] During the fabric laying process, the average laying height of the mixed sintering material is 900mm.

[0037] Example 1

[0038] A method for enhancing flue gas recirculation sintering includes the following steps:

[0039] 1) Ore blending: The ore is blended according to the following mass percentages: bentonite 0.5%, mixed iron ore 60.5% (the mass percentage of particles with a particle size of -0.5mm is <30%, the same below), dolomite 5.5%, limestone 2.5%, quicklime 4.0%, recycled ore 23%, and coke powder 4.0% (to obtain the main chemical composition of sinter: TFe 55.99%, CaO 10.56%, SiO2 5.77%, sinter basicity R = 1.83);

[0040] 2) Granulation: The mixed raw materials are pre-wetted (water content is 6%) and granulated using a cylindrical granulator to obtain sintered mixture. The cylinder speed is 16 rpm, the granulation time is 5 min, and the filling rate is 10%. The average particle size of the obtained granules is 3.3 mm.

[0041] 3) Sintering: Set the ignition temperature to 900℃, ignition time to 5min, and ignition negative pressure to 6kPa; keep the sintering negative pressure constant at 12kPa; and the cooling negative pressure to 6kPa.

[0042] 4) Flue gas recirculation: Head flue gas, middle flue gas, and tail flue gas are drawn from wind boxes No. 1-6, No. 6-26, and No. 27-30 respectively. The tail flue gas with higher temperature in the sintering flue gas is mixed with the hot exhaust gas from the sintering ring cooler and circulated to the front part of the sintering machine through the flue gas hood. The front part is from the ignition point of the sintering machine to the 1 / 2 position of the sintering machine length. The head flue gas with lower temperature in the sintering flue gas and the middle flue gas are mixed and circulated to the rear part of the sintering machine through the flue gas hood. The rear part is from the 1 / 2 position of the sintering machine length to the tail of the sintering machine.

[0043] The tested air volume at the sintering material surface was 41821 Nm. 3 / min, the average CO emission from wind boxes 3-22 was 9139.31 mg / m³. 3 The sintering utilization coefficient is 29.06 t·m. -2 d -1 Vertical sintering speed 22.65 mm·min -1 The sinter drum strength was 77.77%, and the solid fuel consumption was 53.97 kg·t. -1 Compared with the control group, the quality of sintered ore was significantly improved.

[0044] Example 2

[0045] A method for enhancing flue gas recirculation sintering includes the following steps:

[0046] 1) Ore blending: The raw materials are blended according to the following mass percentages: bentonite 1.0%, blended iron ore 60%, dolomite 5.5%, limestone 2.5%, quicklime 4.0%, return ore 23%, and coke powder 4.0% (to obtain the main chemical composition of sinter: TFe 55.51%, CaO 10.91%, SiO2 5.97%, and sinter basicity R = 1.83);

[0047] 2) Granulation: The mixed raw materials are pre-wetted (water content is 5.8%) and granulated using a cylindrical granulator to obtain sintered mixture. The cylinder speed is 16 rpm, the granulation time is 5 min, and the filling rate is 10%. The average particle size of the obtained granules is 3.8 mm.

[0048] 3) Sintering: Set the ignition temperature to 900℃, ignition time to 5min, and ignition negative pressure to 6kPa; sintering negative pressure to be constant at 12kPa; cooling negative pressure to 6kPa.

[0049] 4) Flue gas recirculation: Head flue gas, middle flue gas, and tail flue gas are drawn from wind boxes No. 1-6, No. 6-26, and No. 27-30 respectively. The tail flue gas with higher temperature (200-450℃) in the sintering flue gas is mixed with the hot exhaust gas from the sintering ring cooler and circulated through the flue gas hood to the front part of the sintering machine, which is from the ignition point of the sintering machine to the halfway point of the sintering machine length. The head flue gas with lower temperature (100-150℃) in the sintering flue gas and the middle flue gas are mixed and circulated through the flue gas hood to the rear part of the sintering machine, which is from the halfway point of the sintering machine length to the tail of the sintering machine.

[0050] The tested air volume at the sintering surface was 49773 Nm. 3 / min, the average CO emission from wind boxes 3-22 was 8237.37 mg / m³. 3 The sintering utilization coefficient is 31.39 t·m. -2 d -1 Vertical sintering speed: 23.48 mm / min -1 The sinter drum strength was 79.50%, and the solid fuel consumption was 49.97 kg·t. -1 Compared with the control group, the quality of sintered ore was significantly improved.

[0051] Comparative Example 1

[0052] A method for flue gas recirculation sintering includes the following steps:

[0053] 1) Ore blending: The raw materials are blended according to the following mass percentages: 61% iron ore, 5.5% dolomite, 2.5% limestone, 4.0% quicklime, 23% recycled ore, and 4.0% coke powder (to obtain the main chemical composition of sinter: TFe 55.99%, CaO 10.56%, SiO2 5.77%, and sinter basicity R = 1.83);

[0054] 2) Granulation: The raw materials are pre-wetted (water content is 6.0%) and granulated using a cylindrical granulator to obtain sintered mixture. The cylinder speed is 16 rpm, the granulation time is 5 min, and the filling rate is 10%. The average particle size of the obtained granules is 2.9 mm.

[0055] 3) Sintering: Set the ignition temperature to 900℃, ignition time to 5min, and ignition negative pressure to 6kPa; keep the sintering negative pressure constant at 12kPa; and the cooling negative pressure to 6kPa.

[0056] 4) Flue gas recirculation: Head flue gas, middle flue gas and tail flue gas are drawn from wind boxes No. 1-6, No. 6-26 and No. 27-30 respectively. The head flue gas and tail flue gas are mixed and fed into the hot exhaust gas of the sintering ring cooler and circulated to the sintering machine. The middle flue gas is released after desulfurization and denitrification treatment.

[0057] The tested air volume at the sintering material surface was 28782 Nm. 3 / min, the average CO emission from wind boxes 3-22 is 18746 mg / m³ 3 The sintering utilization coefficient is 23.74 t·m. -2 d -1 Vertical sintering speed: 18.93 mm / min -1 The sinter drum strength was 73.19%, and the solid fuel consumption was 60.43 kg·t. -1 .

[0058] Comparative Example 2

[0059] A method for flue gas recirculation sintering, the steps of which are roughly the same as those in Comparative Example 1, the difference being: ore blending: the raw materials are blended according to the mass percentages of bentonite 0.5%, mixed iron ore 60.5%, dolomite 5.5%, limestone 2.5%, quicklime 4.0%, return ore 23%, and coke powder 4.0% (to obtain the main chemical composition of the sinter: TFe 55.99%, CaO 10.56%, SiO2 5.77%, and sinter basicity R = 1.83).

[0060] The tested air volume at the sintering surface was 32594 Nm. 3 / min, the average CO emission from wind boxes 3-22 was 16594 mg / m³ 3 The sintering utilization coefficient is 26.25 t·m. -2 d -1 Vertical sintering speed: 20.17 mm / min -1 The sinter drum strength was 75.32%, and the solid fuel consumption was 58.47 kg·t. -1 .

[0061] Comparative Example 3

[0062] A flue gas recirculation sintering method, the steps of which are roughly the same as those in Comparative Example 1, the difference being: ore blending: the raw materials are blended according to the mass percentages of bentonite 1.0%, mixed iron ore 60%, dolomite 5.5%, limestone 2.5%, quicklime 4.0%, return ore 23%, and coke powder 4.0% (to obtain the main chemical composition of the sinter: TFe 55.51%, CaO 10.91%, SiO2 5.97%, sinter basicity R = 1.83); the average particle size of the mixture obtained by granulation is 3.8 mm.

[0063] The tested air volume at the sintering material surface was 37173 Nm. 3 / min, average CO emission from wind boxes 3-22 is 15196 mg / m³ 3 The sintering utilization coefficient is 27.95 t·m. -2 d -1 Vertical sintering speed: 21.03 mm / min -1 The sinter drum strength was 76.12%, and the solid fuel consumption was 57.27 kg·t. -1 .

[0064] This invention is not limited to the embodiments described above. Those skilled in the art can make various improvements and modifications without departing from the principles of this invention, and these improvements and modifications are also considered within the scope of protection of this invention. Contents not described in detail in this specification are prior art known to those skilled in the art.

Claims

1. A method for enhancing flue gas recirculation sintering, comprising the steps of batching, granulation, material distribution, and flue gas recirculation sintering, characterized in that, The main steps include: 1) During the batching process, bentonite, iron ore, flux, and fuel are used as the main raw materials, which are mixed and granulated to obtain mixed sintered material; 2) After granulation, the sintering mixture is fed into the sintering machine trolley for flue gas circulation sintering; the specific steps include: dividing the sintering machine into front and rear sections along the trolley's running direction, the front section being from the ignition point of the sintering machine to 1 / 3 to 2 / 3 of the sintering machine's length; the sintering flue gas is divided into head flue gas, middle flue gas, and tail flue gas along the sintering machine's running direction, wherein the head flue gas is taken from the flue gas collected by the bellows located from the ignition point of the sintering machine to 1 / 10 to 1 / 5 of the sintering machine's length, and the tail flue gas refers to the flue gas collected by the bellows located from the tail of the sintering machine to 1 / 10 to 1 / 5 of the sintering machine's length; In the flue gas recirculation step, the tail flue gas in the sintering flue gas is mixed with the hot exhaust gas from the sintering ring cooler and circulated to the front part of the sintering machine through the flue gas hood; the head flue gas and middle flue gas in the sintering flue gas are mixed and circulated to the rear part of the sintering machine through the flue gas hood. The bentonite constitutes 0.1% to 1.0% of the total mass of the mixed sinter. The iron ore accounts for 55-65% of the total mass of the mixed sinter.

2. The method according to claim 1, characterized in that, The main chemical components and their mass percentages in the mixed sintering material include: TFe 55~60%, CaO 8.0~11.0%, and SiO2 4.8~6.0%.

3. The method according to claim 1, characterized in that, The flux is one or more of dolomite, limestone, and quicklime.

4. The method according to claim 1, characterized in that, The fuel is one or more of coke powder and anthracite.

5. The method according to claim 1, characterized in that, Step 1) introduces recycled ore during the batching process, with its content accounting for 20-25% of the total mass of the mixed sinter.

6. The method according to claim 1, characterized in that, The average particle size of the sintered mixture obtained from the granulation step is 3~4 mm.

7. The method according to claim 1, characterized in that, The process parameters used in the flue gas circulation sintering step include: ignition temperature 900~1100℃, ignition time 5~8min, ignition negative pressure 6~8kPa; sintering negative pressure constant 12~13kPa; cooling negative pressure 6~8kPa.

Citation Information

Patent Citations

  • Method for increasing waste gas circulation sintering utilization coefficient and sintered ore barrate strength

    CN102808080A

  • Sintering flue gas circulation method and device

    CN109668444A

  • Pellet roasting system and method based on sintering machine

    CN113604662A