Method for recovering valuable metals from ternary lithium-ion battery positive electrode sheet

By mechanically activating and calcining the positive electrode sheet of ternary lithium-ion batteries, combined with acid solution treatment, the problems of low lithium recovery rate and high reagent consumption in existing technologies have been solved, achieving efficient and economical lithium recovery.

CN118256719BActive Publication Date: 2026-11-24INSTITUTE OF PROCESS ENGINEERING CHINESE ACADEMY OF SCIENCES
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410327150.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-21
Publication Date
2026-11-24
Estimated Expiration
2044-03-21

AI Technical Summary

Technical Problem

Existing ternary lithium-ion battery recycling methods have low lithium recovery rates and require the introduction of large amounts of auxiliary reagents, resulting in low economic efficiency and the generation of waste salt and waste gas.

Method used

By mechanically activating and calcining the positive electrode sheet of a ternary lithium-ion battery, and using the aluminum foil current collector, binder, and conductive agent in the positive electrode sheet as reducing agents, combined with acid leaching treatment with acid solution, in-situ mineral phase deconstruction and selective lithium extraction are achieved, avoiding the use of external calcination aids.

Benefits of technology

It improves lithium yield, reduces reagent consumption and waste emissions, and achieves efficient and economical lithium recovery with a lithium yield of up to 98.5%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118256719B_ABST
    Figure CN118256719B_ABST
Patent Text Reader

Abstract

The application provides a valuable metal recovery method for a ternary lithium ion battery positive plate, and belongs to the technical field of solid waste treatment. The recovery method comprises the following steps: step 1, mechanically activating the ternary lithium ion battery positive plate to obtain activated material; the ternary lithium ion battery positive plate comprises an aluminum foil current collector, a binder and a conductive agent; step 2, roasting the activated material under inert gas protection to obtain roasted material; step 3, mixing the roasted material with an acid solution for acid leaching treatment, and obtaining lithium-containing liquid and solid residue after solid-liquid separation. The application has high lithium yield for the ternary lithium ion battery positive plate, does not need to add roasting aids, and has the advantages of high efficiency and economy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of solid waste treatment technology, specifically relating to a method for recovering valuable metals from the positive electrode sheet of a ternary lithium-ion battery. Background Technology

[0002] Ternary lithium-ion batteries (referred to as ternary batteries) are widely used in electric vehicles due to their high energy density and high voltage platform. However, the number of discarded ternary batteries is increasing year by year. These discarded ternary batteries contain energy metals such as lithium, nickel, and cobalt, making them important secondary resources that urgently need to be utilized. The conventional method for recycling ternary batteries is to first discharge and disassemble the waste batteries, then crush and screen them to separate the current collector and electrode materials, thus obtaining ternary black powder. This black powder is then added to hydrogen peroxide and sulfuric acid to simultaneously leach lithium, nickel, cobalt, and manganese into the solution. Manganese, cobalt, and nickel are then extracted sequentially before lithium is recovered. However, this multi-step extraction and separation process leads to lithium loss, resulting in a low lithium recovery rate from ternary batteries, typically only reaching 70%–85%.

[0003] Existing technologies propose roasting ternary black powder in the presence of additives such as coke, methane, hydrogen, sulfuric acid, and nitric acid to decompose the mineral phase of the cathode material and extract lithium. This can reduce lithium loss to some extent, but the lithium yield still needs to be further improved. Furthermore, existing technologies require the introduction of a large amount of auxiliary reagents, resulting in low economic efficiency and generating significant amounts of waste salt and waste gas. Summary of the Invention

[0004] In view of this, this application provides a method for recovering valuable metals from the positive electrode sheet of a ternary lithium-ion battery. This method has a high lithium recovery rate from the positive electrode sheet of the ternary lithium-ion battery and does not require the addition of external calcination additives, thus having advantages such as high efficiency and economy.

[0005] This application provides a method for recovering valuable metals from the positive electrode sheet of a ternary lithium-ion battery, comprising the following steps: Step 1, mechanically activating the ternary lithium-ion battery positive electrode sheet to obtain activated material; the ternary lithium-ion battery positive electrode sheet includes an aluminum foil current collector, a binder, and a conductive agent; Step 2, calcining the activated material under inert gas protection to obtain calcined material; Step 3, mixing the calcined material with an acid solution for acid leaching treatment, and obtaining lithium-containing liquid and solid residue after solid-liquid separation. This application uses aluminum foil current collectors, binders, and conductive agents in the positive electrode sheet directly or indirectly as reducing agents. Through mechanical activation treatment, the reducing agents are brought into more complete contact with the positive electrode active material, which can improve the reactivity of the reducing agents. During the calcination process, on the one hand, the aluminum foil current collector directly exerts a reducing effect through the aluminothermic reaction, and on the other hand, it is directly reduced by the carbon elements in the conductive agent and binder, or combines with the oxygen elements in the ternary positive electrode active material at high temperature to form carbon monoxide, thus indirectly exerting a reducing effect. By combining the two reduction methods of solid-solid reaction and gas-solid reaction, the ternary positive electrode active material is deconstructed in situ, improving the reduction effect on the valuable metals in the positive electrode sheet, converting lithium into lithium carbonate, lithium aluminate, and lithium fluoride, and converting elements such as nickel and cobalt into elemental or low-valence metal ion forms. The subsequent acid leaching treatment with an acid solution enables selective lithium extraction, separating lithium and other metal elements. This method makes full use of the resources in the positive electrode of ternary lithium-ion batteries, not only avoiding the introduction of additional auxiliary reagents, but also achieving selective extraction of lithium through in-situ mineral phase deconstruction combined with acid leaching treatment, thereby improving the lithium yield and contributing to higher purity of lithium products.

[0006] Preferably, based on the mass of the ternary lithium-ion battery cathode sheet, the total mass content of the aluminum foil current collector, binder, and conductive agent is 15-25%. Controlling the total mass content of the aluminum foil current collector, binder, and conductive agent in the ternary lithium-ion battery cathode sheet within the above range can improve the reduction activity during the calcination process and further increase the lithium yield.

[0007] Preferably, the mass ratio of the aluminum foil current collector, binder, and conductive agent is 1:(0.1-0.3):(0.1-0.2). This application further adjusts the mass ratio of the aluminum foil current collector, binder, and conductive agent within the above range to ensure close cooperation among the three components, thereby improving the reduction effect and achieving a higher lithium yield.

[0008] In some embodiments, based on the mass of the ternary lithium-ion battery cathode sheet, the mass content of the aluminum foil current collector is 10–20.8%, the mass content of the binder is 1.2–5.4%, and the mass content of the conductive agent is 1.1–3.8%.

[0009] In some embodiments, the positive electrode active material is selected from lithium nickel cobalt manganese oxide and / or lithium nickel cobalt aluminum oxide.

[0010] Preferably, the mechanical activation treatment includes at least one of ball milling activation, sand milling activation, and rod milling activation, such as planetary ball milling activation. These activation methods cause the material to break and fracture through mechanical force, thereby increasing the reactivity of the activated material and increasing the contact area of ​​the reactants, thus improving the reduction effect of subsequent roasting treatment.

[0011] Preferably, the mechanical activation treatment time is 6–10 hours. Controlling the mechanical activation treatment time within the above range can obtain components with suitable particle sizes, improve the reduction effect during calcination, and help increase the yield of each element.

[0012] Preferably, in step 2, the calcination temperature is 652–850°C, and the calcination time is 1–4 hours. Calcination at this temperature promotes the aluminothermic reduction and carbon reduction reactions, and also facilitates the formation of carbon monoxide products, further improving the reduction effect, reducing the chemical valence state of the valuable metals in the cathode sheet, and increasing the yield of valuable metals.

[0013] To further improve the lithium yield, the calcination temperature is 700–800°C; for example, the calcination temperature is 700–750°C; and the calcination time is 1–2 hours.

[0014] In some embodiments, the heating rate of the calcination process is 5 to 30 °C / min, for example, 10 °C / min.

[0015] In some embodiments, the inert gas includes nitrogen and / or argon.

[0016] Preferably, in step 3, the acid solution is an aqueous oxalic acid solution; the molar ratio of oxalic acid to the roasted material in the aqueous oxalic acid solution is 1–6 mol / kg. This application utilizes oxalic acid to provide an acidic solution environment, converting poorly water-soluble lithium aluminate, lithium fluoride, and lithium carbonate into lithium oxalate for leaching into the solution, while converting nickel, cobalt, manganese, and / or aluminum into insoluble solids that remain in the solid phase, thereby achieving selective lithium extraction. The combination of oxalic acid within this ratio range with the roasted material allows for better extraction of lithium from the roasted material, further improving the lithium yield.

[0017] In some embodiments, solid slag containing nickel, cobalt, manganese and / or aluminum can be further separated and purified by methods such as acid treatment, electrolysis, ion exchange, and magnetic separation to realize the resource recovery and utilization of valuable metals in the positive electrode sheet.

[0018] Preferably, the oxalic acid concentration in the aqueous oxalic acid solution is 0.5–1 mol / L; the acid leaching treatment time is 10–30 min. This concentration of oxalic acid in the aqueous solution allows for better reaction with the roasted material, and controlling the acid leaching time helps to achieve a higher lithium yield.

[0019] Furthermore, to ensure a more complete reaction of valuable metal elements such as lithium in the roasted material, the oxalic acid concentration is 0.8–1.0 mol / L, and the acid leaching treatment time is 15–20 min.

[0020] Preferably, step 3 further includes: removing impurities from the lithium-containing liquid, and obtaining lithium oxalate after solid-liquid separation; the impurity removal process includes adding a precipitant to the lithium-containing liquid and carrying out a precipitation reaction at a pH of 7-9. By adjusting the pH to 7-9 through the impurity removal process, the aluminum element in lithium oxalate can be converted into aluminum hydroxide precipitate, thereby improving the purity of the lithium oxalate product and achieving higher economic benefits.

[0021] Preferably, the precipitant includes at least one of calcium oxide, calcium carbonate, and calcium hydroxide. Using the above-mentioned precipitant allows for the precipitation of aluminum by adjusting the pH, while simultaneously converting impurity fluorine into calcium fluoride precipitate, further improving the purity and quality of the lithium oxalate product.

[0022] Preferably, the precipitation reaction time is 30–90 min.

[0023] Based on the method for recovering valuable metals from the positive electrode sheet of a ternary lithium-ion battery according to this application, the beneficial effects of the technical solutions provided in some embodiments include at least the following:

[0024] This application achieves the reduction of the positive electrode active material by the self-components of the ternary positive electrode sheet through a combination of mechanical activation and calcination. This reduction and deconstruction of the mineral phase of the positive electrode material can be accomplished without the introduction of external auxiliary reagents, achieving rational use of resources, avoiding excessive reagent consumption and waste, and reducing the emission of waste salts and exhaust gases. Mechanical activation further enhances the activity of the aluminum foil and increases the contact area between the aluminum foil, carbon, and the ternary positive electrode material, thereby strengthening the reaction activity and accelerating the reaction rate. It also increases the contact area between carbon elements in the conductive agent and binder and oxygen elements in the positive electrode active material. The formation of carbon monoxide during calcination further enhances the reduction effect. After calcination, the ternary cathode material is reduced and decomposed, in which lithium is converted into lithium aluminate, lithium carbonate and lithium fluoride. This application uses an acid solution system, preferably an oxalic acid aqueous solution system, to convert lithium into easily soluble lithium oxalate and nickel, cobalt, manganese and / or aluminum into insoluble solids, thereby achieving selective lithium extraction, improving the separation effect and yield of lithium, and having the advantages of low reagent consumption, good selectivity and high lithium yield. Attached Figure Description

[0025] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0026] Figure 1 A flowchart illustrating a method for recovering valuable metals from the positive electrode of a ternary lithium-ion battery, provided for specific embodiments of this application;

[0027] Figure 2 This is a schematic diagram of a specific process flow for a method of recovering valuable metals from the positive electrode sheet of a ternary lithium-ion battery, provided for specific embodiments of this application. Detailed Implementation

[0028] To make the objectives, technical solutions, and advantages of this application clearer, the following detailed description is provided in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application.

[0029] The existing recycling methods for ternary lithium batteries have a low lithium recovery rate. The inventors of this application have discovered that the fluorinated binder and residual fluorinated electrolyte in the positive electrode sheet of waste ternary lithium-ion batteries are prone to generating lithium fluoride during the recycling process. Since lithium fluoride has low solubility in water, it is difficult to dissolve in aqueous solution, which also leads to a decrease in lithium recovery rate.

[0030] Therefore, in response to the problems of large lithium loss, large amount of additives, high cost, and low yield in existing ternary battery cathode recycling methods, this paper refers to... Figure 1 The flowchart shown illustrates a method for recovering valuable metals from the positive electrode sheet of a ternary lithium-ion battery, comprising the following steps: Step 1: Mechanically activating the ternary lithium-ion battery positive electrode sheet to obtain activated material; the ternary lithium-ion battery positive electrode sheet includes an aluminum foil current collector, a binder, and a conductive agent; Step 2: Calcining the activated material under inert gas protection to obtain calcined material; Step 3: Mixing the calcined material with an acid solution for acid leaching treatment, and obtaining lithium-containing liquid and solid residue after solid-liquid separation.

[0031] This application selects waste ternary lithium battery cathode sheets as the starting material. The cathode sheet includes cathode active material, conductive agent, binder, aluminum foil current collector, and electrolyte. First, mechanical activation is used to break the cathode sheet into powder, which simultaneously enhances the activity of the aluminum foil current collector, allowing for more thorough contact between the reducing agent and the cathode active material. Then, the reducing pyrolysis products of the aluminum foil, conductive agent, and binder in the cathode sheet are used as reducing agents. This allows for in-situ deconstruction of the mineral phase of the cathode material without introducing additional additives, converting lithium into lithium carbonate, lithium aluminate, and lithium fluoride, nickel and cobalt into elemental nickel and cobalt, and manganese into elemental manganese and / or manganese oxide.

[0032] Based on reduction, the method employs an acid solution for selective lithium extraction from the reduced material, leaching lithium aluminate, lithium carbonate, and lithium fluoride into the solution. This selective lithium extraction using an acid solution converts lithium-containing compounds that cannot be extracted by water leaching into more soluble lithium salts, while simultaneously inhibiting the dissolution of nickel, cobalt, and manganese. Compared to conventional methods, the recovery method presented in this application significantly improves the lithium leaching rate and selectivity, achieving rapid and selective extraction of lithium and ensuring a high yield and purity of lithium.

[0033] This application does not specify the types of aluminum foil current collector, binder, and conductive agent used in ternary lithium-ion batteries, as long as the reduction effect can be achieved. In some embodiments, the total mass content of the aluminum foil current collector, binder, and conductive agent is 15-25% based on the mass of the ternary lithium-ion battery positive electrode sheet. Exemplarily, based on the mass of the ternary lithium-ion battery positive electrode sheet, the total mass content of the aluminum foil current collector, binder, and conductive agent can be selected from 15%, 16.5%, 17.2%, 18.6%, 19.3%, 20.6%, 21.5%, 22.3%, 23.7%, 24.5%, 25%, or any two of the above values.

[0034] In some embodiments, based on the mass of the ternary lithium-ion battery positive electrode sheet, the mass content of the aluminum foil current collector is 10-20.8%, for example, selected from 10%, 10.5%, 11.2%, 13.8%, 15.4%, 17.3%, 18.2%, 19.6%, 20.8%, or any two of the above values; the mass content of the binder is 1.2-5.4%, for example, selected from 1.2%, 1.8%, 2.3%, 3.5%, 4.6%, 5.4%, or any two of the above values; the mass content of the conductive agent is 1.1-3.8%, for example, selected from 1.1%, 1.5%, 1.8%, 2.2%, 2.5%, 2.8%, 3.3%, 3.5%, 3.8%, or any two of the above values.

[0035] Reference Figure 2The schematic diagram of the specific process flow shown in this application does not impose any special limitations on the preparation of the positive electrode sheet of the ternary lithium-ion battery. For example, it can be prepared by discharging and dismantling the waste ternary lithium-ion battery to separate the positive electrode sheet, negative electrode sheet and separator.

[0036] Reference Figure 2 The schematic diagram of the specific process flow shown illustrates that, in some embodiments, step 1 further includes: before mechanical activation treatment, shearing the ternary lithium-ion battery positive electrode sheet to control the longest diameter of the ternary lithium-ion battery positive electrode sheet to be 0.5–2 cm. Within this range of the longest diameter, it is beneficial to improve the effect of subsequent mechanical activation treatment of the positive electrode sheet.

[0037] Reference Figure 2 The schematic diagram of the specific process flow shown includes, in some embodiments, step 1: mechanically activating the ternary lithium-ion battery positive electrode sheet to obtain activated powder (equivalent to the aforementioned activated material).

[0038] In some embodiments, the mechanical activation treatment time is 6–10 hours. Exemplarily, the mechanical activation treatment time is 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, or any combination of two of these values. This application controls the mechanical activation treatment time within the above range, resulting in good activation effect, which can sufficiently improve the reduction activity of the aluminum foil, increase the contact area between aluminum and the positive electrode active material, and enhance the reaction rate. If the mechanical activation time is too short, the aluminum foil particle size will not be small enough, resulting in insufficient activation effect and thus negatively impacting reaction activity. If the mechanical activation treatment time is too long, it is not conducive to energy conservation and also reduces processing capacity, increasing the risk of agglomeration of the activated material and affecting the reduction effect in the subsequent calcination process.

[0039] In some embodiments, the mechanical activation treatment further includes the addition of an alcohol compound; the alcohol compound includes at least one selected from methanol, ethanol, propanol, ethylene glycol, and glycerol. These alcohol compounds can accelerate the breaking of internal chemical bonds in the material during mechanical activation, improving activation efficiency. Simultaneously, they act as a protective medium coating the surface of the activated material, reducing agglomeration caused by electrostatic forces and preventing safety issues arising from sparks generated during metal grinding.

[0040] In some embodiments, the recycling method further includes: after the mechanical activation treatment in step 1, the activated material is dried to remove alcohol compounds.

[0041] Reference Figure 2 The schematic diagram of the specific process flow shown includes, in some embodiments, step 2: calcining the activated powder under inert gas protection to obtain calcined powder (equivalent to the aforementioned calcined material).

[0042] In some embodiments, in step 2, the calcination temperature is 652–850°C; the calcination time is 1–4 hours. Exemplarily, the calcination temperature is 652°C, 660°C, 670°C, 690°C, 700°C, 710°C, 730°C, 750°C, 760°C, 800°C, 850°C, or any combination of two of the above values. Exemplarily, the calcination time is 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, or any combination of two of the above values.

[0043] Reference Figure 2 The schematic diagram of the specific process flow shown includes, in some embodiments, step 3: mixing the roasted powder with an oxalic acid aqueous solution for selective lithium extraction (equivalent to the aforementioned acid leaching treatment), and obtaining lithium extraction liquid (equivalent to the aforementioned lithium-containing liquid) and lithium extraction slag (equivalent to the aforementioned solid slag) after solid-liquid separation.

[0044] In some embodiments, in step 3, the acid solution is an aqueous oxalic acid solution; the molar mass ratio of oxalic acid in the aqueous oxalic acid solution to the roasted material is 1–6 mol / kg. Exemplarily, the molar mass ratio of oxalic acid in the aqueous oxalic acid solution to the roasted material is 1 mol / kg, 1.5 mol / kg, 2 mol / kg, 2.5 mol / kg, 3 mol / kg, 3.5 mol / kg, 4 mol / kg, 4.5 mol / kg, 5 mol / kg, 5.5 mol / kg, 6 mol / kg, or any combination of two of the above values.

[0045] In some embodiments, the oxalic acid concentration in the aqueous oxalic acid solution is 0.5–1 mol / L; the acid leaching treatment time is 10–30 min. Exemplarily, the oxalic acid concentration in the aqueous oxalic acid solution is 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1.0 mol / L, or any combination of two of the above values. Exemplarily, the leaching time is 10 min, 15 min, 20 min, 25 min, 30 min, or any combination of two of the above values.

[0046] In some embodiments, the liquid-to-solid ratio of the oxalic acid aqueous solution to the calcined material is 2–6 mL / g. Exemplarily, the liquid-to-solid ratio of the oxalic acid aqueous solution to the calcined material is 2 mL / g, 3 mL / g, 4 mL / g, 5 mL / g, 6 mL / g, or a range consisting of any two of the above values.

[0047] Reference Figure 2 The schematic diagram of the specific process flow shown includes, in some embodiments, step 3 further comprising: removing impurities from the lithium-containing liquid and crystallizing it. For example, the lithium-containing liquid may be subjected to impurity removal treatment, and after solid-liquid separation, a lithium oxalate solution may be obtained. Then, the lithium oxalate solution may be evaporated and crystallized to obtain the lithium oxalate product.

[0048] In some embodiments, step 3 further includes adding an adsorption resin to the lithium oxalate solution to remove trace amounts of calcium ions remaining in the lithium oxalate solution, thereby further improving the purity of the lithium oxalate product.

[0049] The solution of this application will be described below with reference to the following specific embodiments. Unless otherwise specified, the raw materials used in the following embodiments are all from commercially available products, and the devices or equipment used are all purchased from conventional market sales channels.

[0050] Example 1

[0051] The method for recovering valuable metals from the positive electrode sheet of a ternary lithium-ion battery in this embodiment includes the following steps:

[0052] Step 1: Discharge and disassemble the waste nickel-cobalt-manganese lithium ternary batteries to obtain positive electrode sheets, negative electrode sheets, and a lightweight separator; the positive electrode sheet includes an aluminum foil current collector, a binder, and a conductive agent. Based on the mass of the positive electrode sheet, the mass content of the aluminum foil current collector is 15%, the mass content of the binder is 3.7%, and the mass content of the conductive agent is 2.4%.

[0053] The positive electrode sheet is cut to a maximum diameter of 0.5-2 cm. 1 kg of the cut positive electrode sheet is placed into a planetary ball mill and mechanically activated by planetary ball milling at a speed of 400 rpm for 6 hours to obtain activated material.

[0054] Step 2: Place the activated material obtained in Step 1 into a tube furnace, introduce nitrogen as a protective atmosphere, and perform calcination under nitrogen protection. The temperature is increased to 700℃ at a heating rate of 10℃ / min, and the calcination time is controlled to be 1 hour. After cooling, the calcined material is obtained.

[0055] Step 3: Add the roasted material obtained in Step 2 to an oxalic acid aqueous solution with a concentration of 0.7 mol / L. Control the liquid-to-solid ratio of the oxalic acid aqueous solution to the roasted material to be 3 mL / g, which means the molar mass ratio of oxalic acid in the oxalic acid aqueous solution to the roasted material is 2.1 mol / kg. Perform acid leaching treatment at room temperature for 20 min. After the reaction, filter and wash to obtain a lithium oxalate solution and solid residue. The leaching rates of each metal after acid leaching treatment were measured to be 98.5% for lithium, 0.2% for nickel, 0.2% for cobalt, and 0.5% for manganese.

[0056] The above lithium oxalate solution was adjusted to pH=8 by adding calcium oxide. Under this condition, impurity removal was performed to convert the fluorine and aluminum elements in the lithium oxalate solution into calcium fluoride and aluminum hydroxide precipitates and remove them. After reacting for 60 minutes, the solution was evaporated and crystallized to obtain the lithium oxalate product.

[0057] The recovery methods of Examples 2-7 and Comparative Examples 1-3 differ from those of Example 1 only in that the mechanical activation time, roasting temperature, roasting time, molar mass ratio of oxalic acid to roasted material, oxalic acid concentration in the oxalic acid aqueous solution, and / or acid leaching time are changed. The specific operating parameters changed in each example or comparative example and the leaching rate results of each metal are shown in Table 1 below.

[0058] Table 1

[0059]

[0060] As shown in Table 1, the recycling method of this application, through a combination of mechanical activation, roasting and acid leaching, can achieve in-situ mineral phase decomposition of ternary cathode active materials without the use of external reducing agents, realize the recovery and separation of valuable metals in ternary cathode sheets, and obtain extremely high lithium element yield, which has the advantages of high efficiency and economy.

[0061] In this application, the mechanical activation treatment time is controlled to be 6 to 10 hours, which can obtain components with suitable particle size, improve the reduction effect in the roasting treatment, and help improve the yield of each element, and achieve a high leaching rate for lithium metal.

[0062] This application, by controlling the calcination temperature to 652–850°C and the calcination time to 1–4 hours, can promote the aluminothermic reduction and carbon reduction reactions, and also facilitate the formation of carbon monoxide products, further improving the reduction effect, reducing the chemical valence state of valuable metals in the cathode sheet, and increasing the yield of valuable metals. Furthermore, by controlling the calcination temperature to 700–850°C, this application can achieve even better reduction effects and a higher leaching rate of lithium metal.

[0063] This application utilizes oxalic acid to provide an acidic solution environment, converting poorly water-soluble lithium aluminate, lithium fluoride, and lithium carbonate into lithium oxalate for leaching into the solution. Meanwhile, nickel, cobalt, manganese, and / or aluminum are converted into insoluble solids and remain in the solid phase, thus achieving selective lithium extraction. When the molar ratio of oxalic acid in the oxalic acid aqueous solution to the roasted material is controlled at 1–6 mol / kg, the combination of oxalic acid and roasted material within this range allows for better extraction of lithium from the roasted material. Furthermore, controlling the molar ratio of oxalic acid in the oxalic acid aqueous solution to the roasted material at 1.8–6 mol / kg can further improve the lithium yield.

[0064] Compared to Example 1, Comparative Example 1 did not perform mechanical activation before calcination; the sheared positive electrode material was directly placed into the furnace for calcination and deconstruction. Since the mechanical activation described in this application can significantly reduce the size of the electrode and increase the contact area, it is beneficial for the subsequent reduction and deconstruction of the mineral phase of the positive electrode material during the calcination process. Because Comparative Example 1 did not perform mechanical activation on the positive electrode, the lithium leaching rate was only 46.5% under the same calcination and leaching conditions, significantly lower than the 98.5% lithium leaching rate in Example 1, resulting in a significantly reduced lithium recovery rate.

[0065] Compared with Example 1, Comparative Example 2 did not calcine the activated powder, resulting in the ternary material's mineral phase not being decomposed, and lithium still mainly existing in the form of lithium nickel cobalt manganese oxide, which significantly reduced the lithium recovery rate.

[0066] Compared with Example 1, Comparative Example 3 did not introduce oxalic acid solution during the leaching process, and only used aqueous solution as leaching reagent. As a result, it could not efficiently extract the poorly soluble lithium aluminate and lithium fluoride from the roasted powder, leading to a significant decrease in lithium recovery rate.

[0067] Table 2

[0068] serial number Precipitator pH Sedimentation time (min) Lithium oxalate purity % Fluorine content % Aluminum content % Example 1 Calcium oxide 8 60 99.8 0.02 0.01 Example 8 calcium hydroxide 9 30 99.2 0.03 0.02 Comparative Example 4 \ \ \ 89.3 2.5 3.5

[0069] As shown in Table 2, the pH of lithium oxalate is adjusted to 7-9 using the aforementioned precipitant, which converts aluminum into aluminum hydroxide precipitate and fluorine impurity into calcium fluoride precipitate, thereby further improving the purity of the lithium oxalate product. In Comparative Example 4, calcium oxide was not added to remove fluoride and aluminum, resulting in lithium oxalate containing some lithium fluoride and lithium aluminate, leading to lower product purity.

[0070] The above are merely preferred embodiments of this application and are not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the principles of this application should be included within the protection scope of this application.

Claims

1. A method for recovering valuable metals from the positive electrode sheet of a ternary lithium-ion battery, characterized in that, Includes the following steps: Step 1: Mechanically activate the ternary lithium-ion battery positive electrode sheet to obtain activated material; the ternary lithium-ion battery positive electrode sheet includes aluminum foil current collector, binder and conductive agent; the mechanical activation treatment time is 6~10 h, and alcohol compounds are added during the mechanical activation treatment; Step 2: The activated material is calcined under inert gas protection to obtain calcined material; the calcination temperature is 652~850℃. Step 3: Mix the roasted material with an acid solution for acid leaching treatment, and obtain lithium-containing liquid and solid residue after solid-liquid separation; the acid solution is an oxalic acid aqueous solution; the molar mass ratio of oxalic acid in the oxalic acid aqueous solution to the roasted material is 1~6 mol / kg.

2. The recycling method according to claim 1, characterized in that, Based on the mass of the ternary lithium-ion battery cathode sheet, the total mass content of the aluminum foil current collector, binder, and conductive agent is 15-25%.

3. The recycling method according to claim 2, characterized in that, The mass ratio of the aluminum foil current collector, binder, and conductive agent is 1:(0.1~0.3):(0.1~0.2).

4. The recycling method according to any one of claims 1 to 3, characterized in that, The mechanical activation treatment includes at least one of ball milling activation, sand milling activation, and rod milling activation; and / or, The alcohol compounds include at least one of methanol, ethanol, propanol, ethylene glycol, and glycerol.

5. The recycling method according to any one of claims 1 to 3, characterized in that, In step 2, the roasting process takes 1 to 4 hours.

6. The recycling method according to claim 5, characterized in that, The calcination temperature is 700~800℃; the calcination time is 1~2 h; and / or the inert gas includes nitrogen and / or argon.

7. The recycling method according to claim 1, characterized in that, The oxalic acid concentration in the oxalic acid aqueous solution is 0.5~1 mol / L; the acid leaching treatment time is 10~30 min.

8. The recycling method according to claim 1, characterized in that, Step 3 further includes: removing impurities from the lithium-containing liquid and obtaining lithium oxalate after solid-liquid separation; The impurity removal process includes adding a precipitant to the lithium-containing liquid and carrying out a precipitation reaction at a pH of 7 to 9.

9. The recycling method according to claim 8, characterized in that, The precipitant includes at least one of calcium oxide, calcium carbonate, and calcium hydroxide; and / or, The precipitation reaction takes 30 to 90 minutes.

Citation Information

Patent Citations

  • Method for recycling valuable metal from waste lithium ion battery positive electrode powder

    CN112877548A

  • Clean closed-loop recovery method for ternary lithium battery waste

    CN116936985A