Preparation method of high-strength and high-elasticity PtAg alloy

By combining planetary ball mill powder mixing with vacuum melting and positive pressure casting with heat transfer oil cooling, the problems of uneven composition and internal defects in the preparation of PtAg alloys were solved, achieving efficient preparation and improved processing performance of high-strength and high-elasticity PtAg alloys.

CN118256763BActive Publication Date: 2026-11-24GUIYAN CHEM MATERIALS (YUNNAN) CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410503358.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-25
Publication Date
2026-11-24
Estimated Expiration
2044-04-25

AI Technical Summary

Technical Problem

Existing technologies are insufficient for preparing high-strength, high-elasticity PtAg alloys. Problems include gravity segregation, long melting time, uneven composition, complex cooling process, and difficult processing, resulting in numerous internal defects in the ingots and low yield.

Method used

By employing a planetary ball mill for powder mixing, vacuum high-frequency or medium-frequency melting furnace positive pressure suction casting combined with heat transfer oil cooling of the steel mold, the powders of Pt, Ag and rare earth elements are uniformly mixed. Dense ingots are then prepared by positive pressure suction casting, ultimately producing high-strength and high-elasticity PtAg alloy wire.

Benefits of technology

This method improves the uniformity and density of PtAg alloy composition, reduces processing losses, increases material utilization, reduces internal defects in ingots, and enhances processing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118256763B_ABST
    Figure CN118256763B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a high-strength, high-elasticity PtAg alloy. The material comprises 74.9–99% Pt, 1–24.9% Ag, and 0.1–0.2% rare earth elements, which can be one or two of Ce, La, and Sc. The method includes: 1) ball milling and mixing Pt, Ag, and rare earth powders, followed by briquetting; 2) vacuum melting and positive pressure casting to obtain a dense ingot; 3) conventional ingot processing to finally obtain the desired material size. This invention uses ball milling to ensure thorough mixing of the material components, resulting in a more uniform composition and lower melting temperature. Simultaneously, the use of vacuum positive pressure casting produces a dense ingot. The casting mold uses heat-conducting oil to cool the steel mold, which is heated to 250–280°C, allowing for the production of larger ingots, significantly reducing processing losses, and improving material utilization. The addition of rare earth elements improves the tensile strength and elastic modulus of the alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a high-strength, high-elasticity PtAg alloy used as a tension wire in precision meters, and particularly to a method for preparing a PtAg alloy suspension wire material used in accelerometers in inertial navigation systems. Background Technology

[0002] Since the Soviet Union successfully developed PtAg20 and PtAg25 alloys in the 1960s, PtAg alloys have attracted much attention as a high-performance elastic alloy. Platinum-silver (Pt-Ag) alloys possess high tensile strength, high elasticity, low electrical resistance, non-magnetic properties, low thermoelectric potential, low elastic aftereffect, excellent corrosion resistance, and oxidation resistance. They are widely used as tension wires in precision meters, and especially as suspension wires in accelerometers in inertial navigation systems, playing a crucial role in aerospace and other fields. They are hailed as "ace" elastic materials and are also recognized by scholars both domestically and internationally as one of the most difficult alloys to machine. The main reasons for this are: 1) The significant difference in specific gravity between platinum and silver makes conventional melting methods prone to gravity segregation during casting; 2) Platinum's melting point is much higher than silver's, and prolonged melting time can cause severe silver volatilization, affecting the compositional balance of the platinum-silver alloy; 3) The microstructure transformation during the cooling process of platinum-silver alloys is complex, involving peritectic reactions, eutectoid transformations, and ordered transformations. Rapid cooling is necessary to ensure compositional uniformity and reduce the occurrence of various segregation phenomena. However, during rapid cooling, the solid-liquid points of the PtAg alloy differ significantly (see...). Figure 1 For example, PtAg25 alloy has a solid-liquid phase line difference of nearly 200°C. During the solidification process of the melt, it is in the solid-liquid two-phase region for a long time, with poor mobility and difficulty in feeding. This results in a lot of macroscopic and microscopic porosity defects inside the ingot, making the ingot difficult to process; 4) Silver has a strong gas absorption phenomenon, especially when smelted at higher temperatures, this phenomenon is more obvious.

[0003] Currently, the preparation of platinum-silver alloys mainly involves vacuum high-frequency induction melting furnace melting, water-cooled copper mold casting, and homogenization annealing of the ingots before processing. This process is time-consuming, has a low yield, and is not suitable for the stable mass production of platinum-silver alloy wires. Summary of the Invention

[0004] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for preparing high-strength and high-elasticity PtAg alloy. The method involves first weighing high-purity powders of Pt, Ag and rare earth elements according to the required alloy weight percentage, then placing them in a planetary ball mill and milling them under inert gas protection. Finally, a water-cooled steel mold heated by heat transfer oil and a suction casting method using positive pressure of inert gas combined with negative pressure suction are used to prepare a PtAg alloy with superior comprehensive performance.

[0005] Specifically, the present invention provides a method for preparing a high-strength, high-elasticity PtAg alloy, comprising the following steps:

[0006] Step 1: Weigh Pt powder, Ag powder, and rare earth element powder according to their weight percentages, and place them in a planetary ball mill. Fill the milling jar with inert gas and mill. The rare earth element can be one or two of Ce, La, Sm, and Sc, preferably Sc. The inert gas can be nitrogen or argon, preferably argon.

[0007] Step 2: Press the powder material obtained in Step 1 into small pieces to facilitate feeding during smelting and reduce smelting losses.

[0008] Step 3: Add the small pieces obtained in Step 2 into a crucible in a vacuum high-frequency or medium-frequency melting furnace. The crucible material can be high-purity, high-density, high-strength graphite or boron nitride, preferably a high-purity boron nitride crucible. Evacuate the furnace to a vacuum level ≤10. -3 Pa, inert gas is introduced to 0.06-0.08 MPa. Melting temperature is 1580-1600℃, and the material is held at this temperature for 3-5 minutes after it has completely melted.

[0009] Step 4: Lift the stopper rod, open the inert gas filling valve to introduce inert gas, and open the vacuum solenoid valve. These three actions are performed simultaneously to achieve positive pressure suction casting. The pressure difference for suction casting is 5-10 MPa. Positive pressure suction casting into the steel mold yields a Φ15mm ingot, which is dense.

[0010] The stopper rod can be made of high-purity, high-density, high-strength graphite or boron nitride, with high-purity boron nitride being preferred.

[0011] The inert gas is introduced by opening the inert gas charging valve, and the pressure of the inert gas is 0.11 to 0.13 MPa.

[0012] The steel mold is a heat-conducting oil-cooled steel mold, and circulating heat-conducting oil heated to 250-280°C is introduced into the oil-cooling jacket of the steel mold.

[0013] Step 5: Process the ingot obtained in Step 4 to finally obtain wire with a diameter of 0.02mm.

[0014] The advantages of this invention are:

[0015] (1) High-purity Pt powder, Ag powder and rare earth element powder are put into a planetary ball mill. Through long-term powder mixing, Pt and Ag components can be fully mixed and evenly distributed, avoiding the tendency of conventional smelting methods to form specific gravity segregation during casting due to the large difference in specific gravity between platinum and silver.

[0016] (2) Pressing into small pieces and placing them in a crucible for positive pressure casting in a vacuum high-frequency or medium-frequency melting furnace can produce high-density ingots and can melt ingots weighing more than 1 kg. Heat treatment can be performed after 20% to 30% of the processing deformation, and finally wire of the required size can be produced, which improves the utilization rate of materials. In contrast, the traditional preparation of platinum-silver alloys mostly involves placing high-purity single metals of Pt and Ag into a vacuum high-frequency induction melting furnace for melting and casting in a water-cooled copper mold. The resulting ingots are loose, with a maximum weight of only about 300 g. Subsequent processing only requires 5% to 10% of the processing deformation before heat treatment, and the processing is difficult and the material loss is high.

[0017] (3) The casting mold is a heat-conducting oil-cooled steel mold. The ingot cooling starts from the center and spreads to the surrounding area, which improves the problem of difficulty in feeding when casting with traditional water-cooled copper mold, resulting in more macroscopic and microscopic porosity defects inside the ingot.

[0018] (3) By adding rare earth elements, the tensile strength and elasticity of the alloy have been improved to a certain extent.

[0019] (4) The present invention will be further illustrated by the following specific embodiments. The embodiments do not achieve different contents of Pt, Ag and rare earth elements, but the description of the contents of Pt, Ag and rare earth elements based on the present invention is within the protection scope of the present invention. Attached Figure Description

[0020] Figure 1 Binary phase diagram of PtAg alloy.

[0021] Figure 2 Microscopic morphology of platinum-silver 25 alloy ingots prepared by traditional methods at 50x magnification.

[0022] Figure 3 Schematic diagram of vacuum melting positive pressure suction casting.

[0023] Figure 4 Example 1: 50x magnification microstructure of PtAg25CeLa ingot

[0024] Figure 5 Example 2: 50x magnification microstructure of PtAg25Sc ingot.

[0025] Figure 6 Example 3: 50x magnification of PtAg20CeLa ingot.

[0026] Figure 7 Example 4: 50x magnification of PtAg20Sc ingot. Detailed Implementation

[0027] See Figure 3 A method for preparing a high-strength, high-elasticity PtAg alloy includes the following steps:

[0028] Step 1: Weigh Pt powder, Ag powder, and rare earth element powder with a purity ≥ 99.95% by weight, and place them in a planetary ball mill. Fill the milling jar with inert gas and mill for 12 hours. The rare earth element can be one or two of Ce, La, Sm, and Sc, preferably Sc. The inert gas can be nitrogen or argon with a purity of 99.999%, preferably argon.

[0029] Step 2: Press the powder material obtained in Step 1 into small pieces to facilitate feeding during smelting and reduce smelting losses.

[0030] Step 3: Add the small pieces obtained in Step 2 into a crucible in a vacuum high-frequency or medium-frequency melting furnace. The crucible material can be high-purity, high-density, high-strength graphite or boron nitride, preferably a high-purity boron nitride crucible. Evacuate the furnace to a vacuum level ≤10. -3 The pressure is increased to 0.06–0.08 MPa by introducing 99.999% pure argon gas. The melting temperature is 1580–1600℃, and the material is held at this temperature for 3–5 minutes after it has completely melted.

[0031] Step 4: Lift the stopper rod, open the inert gas filling valve to introduce inert gas, and open the vacuum solenoid valve. These three actions are performed simultaneously to achieve positive pressure suction casting. The positive pressure suction casting into the steel mold yields a Φ15mm ingot, which is dense.

[0032] The stopper rod can be made of high-purity, high-density, high-strength graphite or boron nitride, with high-purity boron nitride being preferred.

[0033] The inert gas is introduced by opening the inert gas filling valve. The inert gas can be nitrogen or argon with a purity of 99.999%, preferably argon. The pressure of the inert gas is 0.11 to 0.13 MPa.

[0034] The steel mold is a heat-conducting oil-cooled steel mold, and circulating heat-conducting oil heated to 250-280°C is introduced into the oil-cooling jacket of the steel mold.

[0035] Step 5: Process the ingot obtained in step 4 according to the usual processing technology in this field to finally obtain wire with a diameter of 0.02mm.

[0036] Example 1

[0037] Weigh out 374.5g of Pt powder with a purity of 99.99%, 124.5g of Ag powder with a purity of 99.99%, and 1g of Ce+La powder with a purity of 99% (50% each). Place them in a planetary ball mill, fill with argon gas, and ball mill for 12 hours.

[0038] The powder obtained above is pressed into small pieces and added to a crucible in a vacuum melting furnace. The crucible is made of high-purity boron nitride.

[0039] Evacuate to a vacuum level ≤10 -3 Pa, fill with high-purity argon gas to a pressure of 0.07 Pa, start the power supply and heat to 1580℃, and hold at that temperature for 3 minutes after all the material has melted.

[0040] Simultaneously lift the stopper rod, open the inflation valve to fill with argon gas at a pressure of 0.11 MPa, and open the vacuum solenoid valve to evacuate the vacuum tank to a vacuum level of ≤5 × 10. -3 Pa.

[0041] Positive pressure suction casting yielded dense PtAg25RE ingots with a diameter of 15mm. The heat transfer oil temperature of the steel mold was 250℃.

[0042] PtAg25CeLa wire with a diameter of 0.02 mm was prepared according to conventional processing methods in this field, and the material has good processing performance.

[0043] Example 2

[0044] Weigh out 374.5g of Pt powder with a purity of 99.99%, 124.5g of Ag powder with a purity of 99.99%, and 1g of Sc powder with a purity of 99%. Place them in a planetary ball mill, fill with argon gas, and ball mill for 12 hours.

[0045] The powder obtained above is pressed into small pieces and added to a crucible in a vacuum melting furnace. The crucible is made of high-purity boron nitride.

[0046] Pull the vacuum to a vacuum level ≤10 -3 Pa, fill with high-purity argon gas to a pressure of 0.07 Pa, start the power supply and heat to 1580℃, and hold at that temperature for 3 minutes after all the material has melted.

[0047] Simultaneously lift the stopper rod, open the inflation valve to fill with argon gas at a pressure of 0.11 MPa, and open the vacuum solenoid valve to evacuate the vacuum tank to a vacuum level ≤5 × 10. -3 Pa.

[0048] Positive pressure suction casting yielded dense PtAg25RE ingots with a diameter of 15mm. The heat transfer oil temperature of the steel mold was 265℃.

[0049] PtAg25Sc wire with a diameter of 0.02 mm was prepared using conventional processing methods in this field, and the material exhibits good processing performance.

[0050] Example 3

[0051] Weigh out 399.5g of Pt powder with a purity of 99.99%, 99.5g of Ag powder with a purity of 99.99%, and 1g of Ce+La powder with a purity of 99% (each accounting for 50%), put them into a planetary ball mill, fill with argon gas, and ball mill for 12 hours.

[0052] The powder obtained above is pressed into small pieces and added to a crucible in a vacuum melting furnace. The crucible is made of high-purity boron nitride.

[0053] Pull the vacuum to a vacuum level ≤10 -3 Pa, fill with high-purity argon gas to a pressure of 0.07 Pa, start the power supply and heat to 1600℃, and hold at that temperature for 5 minutes after all the material has melted.

[0054] Simultaneously lift the stopper rod, open the inflation valve to fill with argon gas at a pressure of 0.15 MPa, and open the vacuum solenoid valve to evacuate the vacuum tank to a vacuum level ≤7 x 10. -3 Pa.

[0055] Positive pressure suction casting yielded dense PtAg20Sc ingots with a diameter of 15mm. The heat transfer oil temperature of the steel mold was 280℃.

[0056] PtAg20CeLa wire with a diameter of 0.02 mm was prepared according to conventional processing methods in the field, and the material has good processing performance.

[0057] Example 4

[0058] Weigh out 399.5g of Pt powder with a purity of 99.99%, 99.5g of Ag powder with a purity of 99.99%, and 1g of Sc powder with a purity of 99%. Place them in a planetary ball mill, fill with argon gas, and ball mill for 12 hours.

[0059] The powder obtained above is pressed into small pieces and added to a crucible in a vacuum melting furnace. The crucible is made of high-purity boron nitride.

[0060] Pull the vacuum to a vacuum degree of ≤10-3Pa, fill with high-purity argon gas to a pressure of 0.07Pa, start the power supply and heat to 1600℃, and hold at that temperature for 5 minutes after all the material has melted.

[0061] Simultaneously lift the stopper rod, open the inflation valve to fill with argon gas at a pressure of 0.15 MPa, and open the vacuum solenoid valve to evacuate the vacuum tank to a vacuum level of ≤5 × 10⁻³ Pa.

[0062] Positive pressure suction casting yielded dense PtAg20Sc ingots with a diameter of 15mm. The heat transfer oil temperature of the steel mold was 280℃.

[0063] PtAg20Sc wire with a diameter of 0.02 mm was prepared according to conventional processing methods in this field, and the material has good processing performance.

[0064] Table 1. Comparison of the properties of materials prepared in Examples 1-4 of the present invention with those prepared by conventional methods.

[0065] Sample Tensile strength / MPa Elastic modulus / GPa PtAg25 2050 200 Example 1 2140 215 Example 2 2260 230 PtAg20 1750 175 Example 3 1780 188 Example 4 1870 193

[0066] Summary: Comparison Figure 2 and Figure 4-7It is evident that the PtAg alloy ingots prepared by traditional methods exhibit a coarse columnar crystal structure with a relatively loose microstructure, numerous micropores, and severe compositional segregation. In contrast, the PtAg alloy ingots prepared using the methods described in Examples 1-4 of this invention exhibit a fine-grained, dense microstructure without significant macroscopic segregation phases or defects. The material properties of the PtAg alloy are shown in Table 1. Comparing the alloys prepared in Examples 1-4 with traditional platinum-silver alloys (i.e., PtAg25 and PtAg20 alloys used as comparative examples in the table), it is clear that the methods described in Examples 1-4 can produce ingots with higher density and can melt ingots weighing over 1 kg. During processing, 20%–30% of the deformation can be removed before heat treatment, resulting in significantly reduced processing losses and improved material utilization after reaching the final wire size.

Claims

1. A method for preparing a high-strength, high-elasticity PtAg alloy, characterized in that, The alloy comprises 74.9%–80.1% Pt, 19.9%–24.9% Ag, and 0.1%–0.2% rare earth elements, the total mass of which is 100%. The rare earth elements include one or two of Ce, La, and Sc. The preparation method includes the following steps: Step 1: Weigh Pt powder, Ag powder and rare earth element powder according to weight percentage, put them into a planetary ball mill, fill the ball mill jar with inert gas, and ball mill; Step 2: Press the powder material obtained in Step 1 into small pieces; Step 3: Add the small pieces of material obtained in Step 2 into the crucible of a vacuum high-frequency or medium-frequency melting furnace, and evacuate the furnace to a vacuum degree ≤10. -3 Pa, inert gas is introduced to 0.06-0.08 MPa; the melting temperature is 1580-1600℃, and the material is kept at that temperature for 3-5 minutes after it has completely melted; Step 4: Lift the stopper rod, open the inert gas filling valve to fill inert gas, and open the vacuum solenoid valve. These three actions are performed simultaneously to achieve positive pressure suction casting. The positive pressure suction casting is then poured into the suction casting mold to obtain a dense ingot with a diameter of 15mm. Step 5: Process the ingot obtained in Step 4 to finally obtain wire with a diameter of 0.02mm; The suction casting mold is a heat-conducting oil-cooled steel mold.

2. The method for preparing a high-strength, high-elasticity PtAg alloy according to claim 1, characterized in that: Circulating heat transfer oil is introduced into the oil-cooled jacket of the steel mold.

3. The method for preparing a high-strength, high-elasticity PtAg alloy according to claim 2, characterized in that: The temperature of the heat transfer oil is 250-280℃.

4. The method for preparing a high-strength, high-elasticity PtAg alloy according to claim 1, characterized in that: The rare earth element mentioned is Sc.

5. The method for preparing a high-strength, high-elasticity PtAg alloy according to claim 1, characterized in that: The inert gas is nitrogen or argon.

6. The method for preparing a high-strength, high-elasticity PtAg alloy according to claim 1, characterized in that: The stopper rod is made of high-purity, high-density, high-strength graphite or boron nitride.

7. The method for preparing a high-strength, high-elasticity PtAg alloy according to claim 1, characterized in that: The crucible material includes high-purity, high-density, high-strength graphite or boron nitride.

8. A method for preparing a high-strength, high-elasticity PtAg alloy according to any one of claims 1-7, characterized in that: In step 4, the pressure of the inert gas introduced by opening the inert gas filling valve is 0.11 to 0.13 MPa.

9. A method for preparing a high-strength, high-elasticity PtAg alloy according to claim 6 or 7, characterized in that: The stopper rod and crucible are made of high-purity, high-density, and high-strength boron nitride.

Citation Information

Patent Citations

  • Platinum-silver series elastic alloy and its preparation method

    CN103589896A

  • Ag alloy target material for OLED and preparation method

    CN113564554A