Tungsten-tantalum-chromium-aluminum high-entropy alloy and preparation method thereof
By preparing a tungsten-tantalum-chromium-aluminum high-entropy alloy coating and depositing a multi-principal-element high-entropy alloy on the substrate using magnetron sputtering technology, the problem of microstructural instability of traditional coatings under high-temperature environments was solved, achieving a core-shell material protection with high corrosion resistance and long service life.
Patent Information
- Application Number
- CN202410378595.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-29
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-03-29
AI Technical Summary
Traditional single-principal-element metal alloy coatings are prone to elemental segregation in high-temperature and complex environments, leading to unstable microstructure and reduced service life of core-shell materials. Existing ceramic and MAX materials have failed to effectively solve the corrosion problem of core-shell materials due to their density and brittleness issues.
A tungsten-tantalum-chromium-aluminum high-entropy alloy is used as the coating material and deposited on the substrate by magnetron sputtering co-sputtering technology to form a uniform multi-principal-element high-entropy alloy coating. The high-entropy effect and hysteresis diffusion effect of W, Ta, Cr and Al elements are combined to improve the corrosion resistance and stability of the coating.
This achievement resulted in a uniform microstructure and excellent mechanical strength in the high-entropy alloy coating, improving the corrosion resistance of the nuclear cladding material, extending the service life of the nuclear reactor, and ensuring its safe and stable operation.
Smart Images

Figure CN118256792B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metallic structural materials, specifically to a tungsten-tantalum-chromium-aluminum high-entropy alloy and its preparation method. Background Technology
[0002] Lead-bismuth fast reactors are important nuclear reactors with high efficiency and excellent nuclear fuel utilization. However, the interaction between the core cladding material and the liquid lead-bismuth coolant leads to material corrosion and loss, limiting their long-term stable operation. Therefore, to improve the corrosion resistance of the core cladding material, coating protection technology is now generally used to prepare a dense barrier layer on the surface of the core cladding material to isolate the lead-bismuth alloy from the corrosive effect of the core cladding material.
[0003] Currently, internationally recognized core cladding coating materials include ceramic materials, MAX materials, and metal alloys. However, ceramic and MAX materials suffer from poor density and high brittleness, resulting in insufficient protective performance. In contrast, metal alloys offer advantages such as high hardness, good ductility and toughness, and high corrosion resistance, and are widely used in coating protection applications. However, traditional metal alloys, containing only one main element, readily form intermetallic compounds with other minor alloying elements. This leads to elemental segregation and other phenomena during long-term service in high-temperature and complex environments, resulting in unstable microstructure and reduced service life.
[0004] Therefore, it is necessary to design a new type of alloy coating to replace the existing single-principal alloy in order to improve the corrosion resistance of nuclear cladding materials and achieve long-term safe operation of nuclear reactors. Summary of the Invention
[0005] To address the problems existing in the prior art, this invention provides a tungsten-tantalum-chromium-aluminum high-entropy alloy and its preparation method. The prepared tungsten-tantalum-chromium-aluminum high-entropy alloy has a uniform microstructure and excellent mechanical strength, effectively improving the service life of the material.
[0006] This invention is achieved through the following technical solution:
[0007] A tungsten-tantalum-chromium-aluminum high-entropy alloy, wherein the atomic percentage of the tungsten-tantalum-chromium-aluminum high-entropy alloy is: (WTaCr) 1-x Al x x = 0.5-8; the tungsten-tantalum-chromium-aluminum high-entropy alloy has a crystal structure, which is a body-centered cubic solid solution.
[0008] Preferably, the thickness of the obtained tungsten-tantalum-chromium-aluminum high-entropy alloy is 3μm to 3.6μm.
[0009] Preferably, the nanoindentation hardness of the tungsten-tantalum-chromium-aluminum high-entropy alloy is 10 GPa to 14 GPa.
[0010] A method for preparing a tungsten-tantalum-chromium-aluminum high-entropy alloy includes the following steps:
[0011] In a vacuum environment, a tungsten-tantalum-chromium-aluminum high-entropy alloy was deposited on a substrate using a WTaCr alloy target and an Al elemental target combined with a magnetron sputtering co-sputtering method.
[0012] The WTaCr alloy target is subjected to DC sputtering with a power supply of 200W; the Al elemental target is subjected to RF sputtering with RF power supplies of 20-160W respectively.
[0013] Preferably, during the magnetron sputtering co-sputtering process, the deposition time is 8500s-11000s.
[0014] Preferably, during the magnetron sputtering co-sputtering process, the deposition gas pressure is 1.0 Pa, the deposition temperature is room temperature, and the substrate rotation speed is 15 r / min.
[0015] Preferably, a high-entropy alloy is deposited on a substrate to a certain thickness, and then vacuum cooled to room temperature to obtain a tungsten-tantalum-chromium-aluminum high-entropy alloy.
[0016] Preferably, the vacuum level of the vacuum environment is less than 4.0 × 10⁻⁶. -4 Pa.
[0017] Preferably, the substrate is first polished and cleaned, and then a tungsten-tantalum-chromium-aluminum high-entropy alloy is deposited on the polished and cleaned substrate.
[0018] Preferably, the cleaning method for the substrate is as follows:
[0019] The polished substrate was ultrasonically cleaned in acetone and alcohol for 10 minutes in sequence, and then dried. The roughness of the polished surface was less than 0.8 nm.
[0020] Compared with the prior art, the present invention has the following beneficial technical effects:
[0021] The tungsten-tantalum-chromium-aluminum high-entropy alloy provided by this invention has a large number of components with equal atomic percentages, resulting in extremely high entropy, low Gibbs free energy, and relatively stable system. Furthermore, the mixing enthalpy can be controlled to form a single-phase solid solution, exhibiting extremely high structural stability. Simultaneously, the alloy has a body-centered cubic structure, providing good high-temperature stability and high thermal stability and resistance to high-temperature oxidation. The W, Ta, Cr, and Al elements readily form a dense oxide film and possess characteristics such as crystal structure, body-centered cubic single phase, high mixing entropy, and hysteretic diffusion, all of which contribute to excellent corrosion resistance. In addition, the four major performance characteristics of the high-entropy alloy—high-entropy effect, cocktail effect, hysteretic diffusion effect, and lattice distortion effect—all contribute to its superior corrosion resistance compared to traditional metal alloys.
[0022] This invention utilizes the advantages of magnetron sputtering technology to control the alloy element content through co-sputtering with different targets, preparing a tungsten-tantalum-chromium-aluminum (WTaCrAl) high-entropy alloy with uniform alloy element distribution, a body-centered cubic crystal structure, and excellent performance. This WTaCrAl high-entropy alloy, as a multi-principal element high-entropy alloy, is composed of multiple elements such as tungsten (W), tantalum (Ta), chromium (Cr), and aluminum (Al). These four elements have extremely high melting points and are all refractory metals, exhibiting excellent high-temperature resistance, corrosion resistance, and mechanical properties. The uniform distribution of these elements in the high-entropy alloy, along with effects such as solid solution strengthening, hysteresis diffusion, and lattice distortion, endows it with excellent comprehensive performance under extreme environments, particularly its stability under high temperature, high radiation, and corrosive conditions. Combining the WTaCrAl high-entropy alloy with magnetron sputtering technology, a high-quality, uniform, and dense high-entropy alloy coating can be prepared, providing excellent corrosion protection for the core cladding material of lead-bismuth fast reactors. This coating not only possesses high-temperature stability and oxidation resistance but also effectively resists the erosion of materials by lead-bismuth coolants, extending the service life of nuclear reactors and improving their safe and stable operation. Attached Figure Description
[0023] Figure 1 The images show the XRD results of the tungsten-tantalum-chromium-aluminum high-entropy alloys of this invention with different aluminum contents.
[0024] Figure 2 The TEM microstructure and diffraction pattern of the tungsten-tantalum-chromium-aluminum high-entropy alloy of the present invention with an aluminum content of 8% are shown.
[0025] Figure 3 EDS elemental distribution diagram of the microstructure of the tungsten-tantalum-chromium-aluminum high-entropy alloy of the present invention with an aluminum content of 8%;
[0026] Figure 4 This is a load-displacement curve of the tungsten-tantalum-chromium-aluminum high-entropy alloy with different aluminum contents according to the present invention;
[0027] Figure 5 The results show the nanoindentation hardness of the tungsten-tantalum-chromium-aluminum high-entropy alloys with different aluminum contents. Detailed Implementation
[0028] The present invention will now be described in further detail with reference to the accompanying drawings. These descriptions are intended to explain the invention and not to limit it.
[0029] A tungsten-tantalum-chromium-aluminum high-entropy alloy, wherein the atomic percentage is: (WTaCr) 1-x Al x x = 0.5-8; the tungsten-tantalum-chromium-aluminum high-entropy alloy has a crystal structure, which is a body-centered cubic solid solution.
[0030] The tungsten-tantalum-chromium-aluminum high-entropy alloy was prepared by magnetron sputtering co-sputtering, and the thickness of the obtained tungsten-tantalum-chromium-aluminum high-entropy alloy was 3μm to 3.6μm; the nanoindentation hardness of the tungsten-tantalum-chromium-aluminum high-entropy alloy was 10GPa to 14GPa.
[0031] This tungsten-tantalum-chromium-aluminum high-entropy alloy is a quaternary high-entropy alloy. Due to the large number of components, it has a high mixing entropy and a low Busch free energy. Furthermore, the tungsten-tantalum-chromium-aluminum high-entropy alloy has a body-centered cubic structure, which provides good high-temperature stability and high thermal stability as well as resistance to high-temperature oxidation. The W, Ta, Cr, and Al elements readily form a dense oxide film and possess characteristics such as crystal structure, body-centered cubic single phase, high mixing entropy, and hysteretic diffusion, which can effectively improve the corrosion resistance of the coating.
[0032] This invention also provides a method for preparing a tungsten-tantalum-chromium-aluminum high-entropy alloy, comprising the following steps:
[0033] A tungsten-tantalum-chromium-aluminum high-entropy alloy was deposited on the substrate using a WTaCr alloy target and an Al elemental target, combined with a magnetron sputtering co-sputtering method. The WTaCr alloy target was subjected to DC sputtering with a power supply of 200W, while the Al elemental target was subjected to RF sputtering with RF power supplies ranging from 20 to 160W.
[0034] This application employs a magnetron sputtering co-sputtering method to deposit WTaCrAl alloy on the substrate surface. The principle is to generate Ar through Ar gas ionization. + Ions, accelerated by the cathode potential, bombard the cathode target (WTaCr and Al), sputtering target atoms and secondary electrons. The target atoms deposit onto the anode substrate in the opposite direction. The secondary electrons, moving perpendicular to the electric and magnetic fields in the orthogonal electromagnetic field, exhibit a rolling trajectory, enhancing collisions with Ar molecules and increasing the probability of Ar ionization. The key advantages of this technology are high ionization rate, fast deposition rate, low operating temperature, and controllable element content, minimizing target element agglomeration and backsputtering phenomena that could lead to microstructure inhomogeneity. Finally, the coating is naturally cooled to room temperature in a high-vacuum deposition chamber to avoid rapid oxidation from air, allowing the deposited atoms to fully diffuse and form the final WTaCrAl alloy.
[0035] A method for preparing a tungsten-tantalum-chromium-aluminum high-entropy alloy includes the following steps;
[0036] Step 1: Clean and polish the substrate to obtain a pretreated substrate.
[0037] Take a single-sided polished monocrystalline silicon substrate and ultrasonically clean it in chemically pure acetone and ethanol for 10 minutes in sequence. Then use warm air to dry it quickly so that the surface is clean and free of stains and dust. The surface roughness of the monocrystalline silicon substrate after ultrasonic treatment is less than 0.8 nm. Ultrasonic cleaning of the polished monocrystalline silicon substrate is beneficial to improving the bonding force between the alloy and the substrate.
[0038] Step 2: In a vacuum environment, WTaCr alloy target and Al elemental target are used for magnetron sputtering co-sputtering to deposit WTaCrAl alloy on the surface of the pretreated substrate.
[0039] First, the ultrasonically cleaned monocrystalline silicon substrate is fixed onto a base plate and automatically conveyed into the magnetron sputtering coating chamber. A vacuum is then evacuated until the back-side vacuum reaches 4.0 × 10⁻⁶. -4 Below Pa,
[0040] Secondly, WTaCrAl alloy was prepared by depositing on a silicon substrate using a magnetron sputtering co-sputtering method;
[0041] The WTaCr alloy target has an atomic ratio of W: 37.8%, Ta: 38.3%, and Cr: 23.9%, with a DC power supply of 200W. The Al elemental target has an RF power supply of 20-160W, a deposition gas pressure of 1.0Pa, a deposition temperature of room temperature, a substrate rotation speed of 15r / min, and a deposition time of 8500s-11000s.
[0042] Step 4: Cool the WTaCrAl alloy to room temperature in the furnace to obtain a tungsten-tantalum-chromium-aluminum high-entropy alloy with a thickness of 3μm to 3.6μm.
[0043] Because sputtered atoms bombard the substrate for a long time during the deposition process, the resulting WTaCrAl alloy has a certain temperature rise. After the deposition is completed, it is fully cooled in the high vacuum coating chamber before being removed, which can ensure that the internal stress of the sample is small and the surface is not oxidized by air.
[0044] Example 1
[0045] A method for preparing a WTaCrAl high-entropy alloy includes the following steps;
[0046] Step 1: The single-crystal silicon substrate was ultrasonically cleaned for 10 minutes each in analytical grade acetone and ethanol, and then dried quickly with warm air.
[0047] Step 2: Fix the single-crystal silicon substrate onto the base plate, and automatically transport it into the magnetron sputtering vacuum coating chamber. Evacuate the chamber until the back vacuum level reaches 4.0 × 10⁻⁶. -4 Below Pa.
[0048] Step 3: Using a WTaCr alloy target and an Al single target, and combining a magnetron sputtering DC and RF power supply co-sputtering method, WTaCrAl alloy is deposited on a single crystal silicon substrate.
[0049] The WTaCr alloy target has an atomic ratio of W: 37.8%, Ta: 38.3%, and Cr: 23.9%, a DC power supply of 200W, and an Al elemental target with a radio frequency power supply of 20W. The deposition gas pressure is 1.0Pa, the deposition temperature is room temperature, the substrate rotation speed is 15r / min, and the deposition time is 10000s.
[0050] Step 4: The WTaCrAl alloy deposited on the single-crystal silicon substrate in Step 3 is naturally cooled to room temperature in a high-vacuum coating chamber for 2-3 hours to obtain a high-entropy alloy of W-42at%Ta-32at%Cr-25.5at%Al-0.5at% with a thickness of 3.4μm.
[0051] The microstructure and mechanical properties of the prepared W-42at%Ta-32at%Cr-25.5at%Al-0.5at% alloy were characterized. The alloy structure is a body-centered cubic structure with uniform distribution of W, Ta, Cr and Al elements. The hardness was measured to be 12.11±2.19GPa under a 10000μN load by nanoindentation.
[0052] Example 2
[0053] A method for preparing a WTaCrAl high-entropy alloy includes the following steps;
[0054] Step 1: The single-crystal silicon substrate was ultrasonically cleaned for 10 minutes each in analytical grade acetone and ethanol, and then dried quickly with warm air.
[0055] Step 2: Fix the single-crystal silicon substrate onto the base plate, and automatically transport it into the magnetron sputtering vacuum coating chamber. Evacuate the chamber until the back vacuum level reaches 4.0 × 10⁻⁶. -4 Below Pa.
[0056] Step 3: Using a WTaCr alloy target and an Al single target, and combining a magnetron sputtering DC and RF power supply co-sputtering method, WTaCrAl alloy is deposited on a single crystal silicon substrate.
[0057] The WTaCr alloy target has an atomic ratio of W: 37.8%, Ta: 38.3%, and Cr: 23.9%, a DC power supply of 200W, and an Al elemental target with a radio frequency power supply of 60W. The deposition gas pressure is 1.0Pa, the deposition temperature is room temperature, the substrate rotation speed is 15r / min, and the deposition time is 10000s.
[0058] Step 4: The WTaCrAl alloy deposited on the single-crystal silicon substrate in Step 3 is naturally cooled to room temperature in a high-vacuum coating chamber for 2-3 hours to obtain a W-41at%Ta-32at%Cr-25at%Al-2at% high-entropy alloy with a thickness of 3.5μm.
[0059] The microstructure and mechanical properties of the prepared W-41at%Ta-32at%Cr-25at%Al-2at% alloy were characterized. The alloy structure was amorphous, and the W, Ta, Cr and Al elements were uniformly distributed. The hardness was measured to be 11.4±0.52GPa under a 10000μN load by nanoindentation.
[0060] Example 3
[0061] A method for preparing a WTaCrAl high-entropy alloy includes the following steps;
[0062] Step 1: The single-crystal silicon substrate was ultrasonically cleaned for 10 minutes each in analytical grade acetone and ethanol, and then dried quickly with warm air.
[0063] Step 2: Fix the single-crystal silicon substrate onto the base plate, and automatically transport it into the magnetron sputtering vacuum coating chamber. Evacuate the chamber until the back vacuum level reaches 4.0 × 10⁻⁶. -4 Below Pa.
[0064] Step 3: Using a WTaCr alloy target and an Al single target, and combining a magnetron sputtering DC and RF power supply co-sputtering method, WTaCrAl alloy is deposited on a single crystal silicon substrate.
[0065] The WTaCr alloy target has an atomic ratio of W: 37.8%, Ta: 38.3%, and Cr: 23.9%, a DC power supply of 200W, and an Al elemental target with a radio frequency power supply of 110W, a deposition gas pressure of 1.0Pa, a deposition temperature of room temperature, a substrate rotation speed of 15r / min, and a deposition time of 9500s.
[0066] Step 4: The WTaCrAl alloy deposited on the single-crystal silicon substrate in Step 3 is naturally cooled to room temperature in a high-vacuum coating chamber for 2-3 hours to obtain a W-41at%Ta-31at%Cr-23at%Al-5at% high-entropy alloy with a thickness of 3.6μm.
[0067] The microstructure and mechanical properties of the prepared W-41at%Ta-31at%Cr-23at%Al-5at% alloy were characterized. The alloy structure was amorphous, and the W, Ta, Cr and Al elements were uniformly distributed. The hardness was measured to be 10.35±0.65GPa under a 10000μN load by nanoindentation.
[0068] Example 4
[0069] A method for preparing a WTaCrAl high-entropy alloy includes the following steps;
[0070] Step 1: The single-crystal silicon substrate was ultrasonically cleaned for 10 minutes each in analytical grade acetone and ethanol, and then dried quickly with warm air.
[0071] Step 2: Fix the single-crystal silicon substrate onto the base plate, and automatically transport it into the magnetron sputtering vacuum coating chamber. Evacuate the chamber until the back vacuum level reaches 4.0 × 10⁻⁶. -4 Below Pa.
[0072] Step 3: Using a WTaCr alloy target and an Al single target, and combining a magnetron sputtering DC and RF power supply co-sputtering method, WTaCrAl alloy is deposited on a single crystal silicon substrate.
[0073] The WTaCr alloy target has an atomic ratio of W: 37.8%, Ta: 38.3%, and Cr: 23.9%, a DC power supply of 200W, and an Al elemental target with a radio frequency power supply of 160W, a deposition gas pressure of 1.0Pa, a deposition temperature of room temperature, a substrate rotation speed of 15r / min, and a deposition time of 8500s.
[0074] Step 4: The WTaCrAl alloy deposited on the single-crystal silicon substrate in Step 3 is naturally cooled to room temperature in a high-vacuum coating chamber for 2-3 hours to obtain a W-40at%Ta-30at%Cr-22at%Al-8at% high-entropy alloy with a thickness of 3.5μm.
[0075] The microstructure and mechanical properties of the prepared W-40at%Ta-30at%Cr-22at%Al-8at% alloy were characterized. The alloy structure was amorphous, and the W, Ta, Cr and Al elements were uniformly distributed. The hardness was measured to be 10.97±1.77GPa under a 10000μN load by nanoindentation.
[0076] Comparative Example
[0077] This comparative study prepared a WTaCr ternary high-entropy alloy.
[0078] A method for preparing a WTaCr high-entropy alloy includes the following steps;
[0079] Step 1: The single-crystal silicon substrate was ultrasonically cleaned for 10 minutes each in analytical grade acetone and ethanol, and then dried quickly with warm air.
[0080] Step 2: Fix the single-crystal silicon substrate onto the base plate, and automatically transport it into the magnetron sputtering vacuum coating chamber. Evacuate the chamber until the back vacuum level reaches 4.0 × 10⁻⁶. -4 Below Pa.
[0081] Step 3: Using a WTaCr alloy target and combining it with a magnetron sputtering DC power supply sputtering method, WTaCrAl alloy is deposited on a single crystal silicon substrate.
[0082] The target atomic ratio of the WTaCr alloy was 37.8%, Ta was 38.3%, and Cr was 23.9%. The DC power supply was 200W, the deposition gas pressure was 1.0Pa, the deposition temperature was room temperature, the substrate rotation speed was 15r / min, and the deposition time was 11000s.
[0083] Step 4: The WTaCr alloy deposited on the single-crystal silicon substrate in Step 3 is naturally cooled to room temperature in a high-vacuum coating chamber for 2-3 hours to obtain a W-30at%Ta-40at%Cr-30at% high-entropy alloy with a thickness of 3.3μm.
[0084] The microstructure and mechanical properties of the prepared W-30at%Ta-40at%Cr-30at% high-entropy alloy were characterized. The alloy structure is a body-centered cubic structure with uniform distribution of W, Ta and Cr elements. The hardness was measured to be 13.85±1.27GPa under a 10000μN load by nanoindentation.
[0085] Figure 1 The figure shows the XRD results of the tungsten-tantalum-chromium-aluminum high-entropy alloy of the present invention with different aluminum contents. Figure 2 The TEM microstructure and diffraction pattern images of the tungsten-tantalum-chromium-aluminum high-entropy alloy of the present invention, with an aluminum content of 8%, are shown. Figure 3 EDS scan elemental distribution diagram of the microstructure of a tungsten-tantalum-chromium-aluminum high-entropy alloy with an aluminum content of 8% is shown. Figure 4 Load-displacement curves of nanoindentation on tungsten-tantalum-chromium-aluminum high-entropy alloys with different aluminum contents are shown. Figure 5 The variation trend of nanoindentation hardness of tungsten-tantalum-chromium-aluminum high-entropy alloys with different aluminum contents is shown.
[0086] The tungsten-tantalum-chromium-aluminum high-entropy alloy of the present invention has a body-centered cubic crystal structure with uniform distribution of alloying elements. As the aluminum content increases, the alloy's hardness gradually decreases, while the indentation depth gradually increases. The tungsten-tantalum-chromium-aluminum high-entropy alloy of the present invention possesses excellent mechanical properties such as high strength and good plastic deformation ability.
[0087] WTaCrAl high-entropy alloy, as a multi-principal-element high-entropy alloy, is composed of a variety of high-melting-point refractory elements such as tungsten (W), tantalum (Ta), chromium (Cr), and aluminum (Al), and has excellent high-temperature resistance. Figure 1 The XRD results show that as the Al content increases, the three orientation peaks of BCC shift to the right, indicating that the lattice distortion increases and the lattice spacing decreases. This helps to reduce vacancies and interstitial spaces, and reduce corrosion channels. Figure 2 High-resolution transmission images show that the microstructure of the WTaCrAl high-entropy alloy is nanocrystalline with a small grain boundary area, which also helps to reduce corrosion channels. Figure 3 The EDS results also showed that the microstructure had a uniform elemental distribution, no intermetallic compounds were formed, the microstructure was a single-phase BCC solid solution, the body-centered cubic structure was stable at high temperatures and had high corrosion resistance. Figure 4 and Figure 5 The alloy exhibits high hardness and elastic modulus, indicating excellent mechanical properties in the coating. This helps the coating maintain its structural integrity during service and enhances its corrosion resistance. Therefore, the uniform distribution of these elements in the high-entropy alloy, along with effects such as solid solution strengthening, hysteresis diffusion, and lattice distortion, endows it with superior comprehensive performance under extreme environments, particularly its stability in high-temperature, high-irradiation, and corrosive environments.
[0088] Magnetron sputtering, as an advanced surface coating preparation method, sprays atoms or molecules from a target surface onto a substrate surface under vacuum conditions to form a dense and uniform coating. This technology offers advantages such as low processing temperature, high coating density, and controllable deposition rate. Compared to traditional thermal spraying, magnetron sputtering causes no thermal damage to the substrate and is less likely to disrupt the coating-substrate interface, making it particularly suitable for coating preparation of nuclear cladding tubes. Therefore, this invention leverages the performance advantages of WTaCrAl high-entropy alloys and combines them with magnetron sputtering technology to deposit a high-quality, uniform, and dense high-entropy alloy coating on the substrate, providing excellent corrosion protection for lead-bismuth fast reactor nuclear cladding materials. This coating not only possesses high-temperature stability and oxidation resistance but also effectively resists the erosion of materials by lead-bismuth coolants, extending the service life of the nuclear reactor and improving its safe and stable operation. Therefore, the application of WTaCrAl high-entropy alloy coating prepared by magnetron sputtering in lead-bismuth fast reactors is of great significance for improving the corrosion resistance of nuclear reactor materials, extending their lifespan, and ensuring their safe operation.
[0089] The above content is only for illustrating the technical concept of the present invention and should not be construed as limiting the scope of protection of the present invention. Any modifications made to the technical solution based on the technical concept proposed in this invention shall fall within the scope of protection of the claims of this invention.
Claims
1. A tungsten-tantalum-chromium-aluminum high-entropy alloy, characterized in that, In the tungsten-tantalum-chromium-aluminum high-entropy alloy, the atomic percentage of W is 42 at, the atomic percentage of Ta is 32 at, the atomic percentage of Cr is 25.5 at, and the atomic percentage of Al is 0.5 at; the tungsten-tantalum-chromium-aluminum high-entropy alloy has a crystal structure, which is a body-centered cubic solid solution.
2. The tungsten-tantalum-chromium-aluminum high-entropy alloy according to claim 1, characterized in that, The thickness of the obtained tungsten-tantalum-chromium-aluminum high-entropy alloy is 3μm~3.6μm.
3. A tungsten-tantalum-chromium-aluminum high-entropy alloy according to claim 1, characterized in that, The nanoindentation hardness of the tungsten-tantalum-chromium-aluminum high-entropy alloy is 10 GPa~14 GPa.
4. A method for preparing a tungsten-tantalum-chromium-aluminum high-entropy alloy according to any one of claims 1-3, characterized in that, Includes the following steps: In a vacuum environment, a tungsten-tantalum-chromium-aluminum high-entropy alloy was deposited on a substrate using a WTaCr alloy target and an Al elemental target combined with a magnetron sputtering co-sputtering method. The WTaCr alloy target is subjected to DC sputtering with a power supply of 200 W; the Al elemental target is subjected to RF sputtering with RF power supplies of 20-160 W respectively.
5. The method for preparing a tungsten-tantalum-chromium-aluminum high-entropy alloy according to claim 4, characterized in that, During the magnetron sputtering co-sputtering process, the deposition time is 8500 s - 11000 s.
6. The method for preparing a tungsten-tantalum-chromium-aluminum high-entropy alloy according to claim 4, characterized in that, During the magnetron sputtering co-sputtering process, the deposition gas pressure is 1.0 Pa, the deposition temperature is room temperature, and the substrate rotation speed is 15 r / min.
7. The method for preparing a tungsten-tantalum-chromium-aluminum high-entropy alloy according to claim 4, characterized in that, A 3.4 μm high-entropy alloy was deposited on the substrate and then vacuum cooled to room temperature to obtain a tungsten-tantalum-chromium-aluminum high-entropy alloy.
8. The method for preparing a tungsten-tantalum-chromium-aluminum high-entropy alloy according to claim 4, characterized in that, The vacuum level of the vacuum environment is less than 4.0 × 10⁻⁶. -4 Pa.
9. A method for preparing a tungsten-tantalum-chromium-aluminum high-entropy alloy according to any one of claims 4-8, characterized in that, First, the substrate is polished and cleaned, and then a tungsten-tantalum-chromium-aluminum high-entropy alloy is deposited on the polished and cleaned substrate.
10. The method for preparing a tungsten-tantalum-chromium-aluminum high-entropy alloy according to claim 9, characterized in that, The cleaning method for the substrate is as follows: The polished substrate was ultrasonically cleaned in acetone and alcohol for 10 minutes in sequence, and then dried.
Citation Information
Patent Citations
NbMoTaWAl refractory high-entropy alloy film and preparation method thereof
CN113151795A
Manufacture of high-tensile cold-rolled steel plate with heat hardenability for deep drawing