Metal complex reducing agent, method of preparation and use thereof
By using the prepared metal complex reducing agent to pickle and immerse the surface of steel parts, the environmental pollution and corrosion problems of traditional pickling methods are solved, realizing a highly efficient and environmentally friendly hot-dip galvanizing process, and improving the quality and durability of the coating.
Patent Information
- Application Number
- CN202410155617.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-04
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-02-04
AI Technical Summary
Traditional pickling methods cause environmental pollution and corrosion problems during hot-dip galvanizing, necessitating the development of more efficient and environmentally friendly pickling technologies.
A metal complexing reducing agent is used to prepare a complexing agent by combining bromoacetic anhydride, triethylenetetramine, a nitrogen-containing organic complexing agent, sodium tripolyphosphate, hexamethylenetetramine, and sodium thiosulfate. The complexing agent is then pickled and immersed on the surface of steel parts, followed by hot-dip galvanizing.
It achieves deep cleaning and uniform treatment of steel surfaces, improves the quality and durability of the coating, reduces chemical loss and corrosion, enhances the adhesion and corrosion resistance of the galvanized layer, and extends the service life of steel parts.
Smart Images

Figure CN118256842B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of hot-dip galvanizing technology, and in particular to a metal complexing reducing agent, its preparation method, and its application. Background Technology
[0002] Hot-dip galvanizing is a crucial corrosion protection method in industrial applications. This technology, by immersing steel products in molten zinc, not only forms a uniform protective layer on their surface but also endows them with excellent corrosion resistance. Particularly in harsh environments, such as those with high salinity, humidity, or strong chemical corrosion, the protective layer provided by hot-dip galvanizing can significantly extend the service life of steel products. Furthermore, due to its uniform and continuous coating characteristics, hot-dip galvanizing also helps prevent rust and corrosion, which is particularly important in fields such as bridge construction, automobile manufacturing, and marine engineering. Through this technology, the overall performance of steel products is enhanced, making them more adaptable to various extreme working conditions.
[0003] The environmental impact of pickling is a critical issue, especially in industrial-scale operations. Acid fumes generated during pickling not only pollute the surrounding environment but also pose a threat to human health. These fumes contain highly corrosive chemicals, such as hydrochloric acid and sulfuric acid, which diffuse into the air, affecting air quality. Furthermore, the treatment and disposal of waste acid generated during pickling is equally serious. If not properly handled, this waste acid can pollute soil and water sources, causing long-term damage to the ecological environment. Therefore, strict environmental protection measures, such as neutralization, safe storage, and disposal, are necessary for the treatment and disposal of pickling waste liquid to minimize environmental impact. In practice, adopting effective exhaust systems to reduce acid fumes and using more environmentally friendly pickling technologies and materials are important measures to reduce the environmental impact of the pickling process.
[0004] Given the problems of traditional pickling methods, such as over-etching and environmental impact, it is necessary to develop more efficient and environmentally friendly pickling technologies. Summary of the Invention
[0005] In view of the above-mentioned deficiencies of the prior art, the technical problem to be solved by the present invention is to provide a metal complex reducing agent, a preparation method thereof and its application.
[0006] This invention provides a complexing agent, prepared by the following method: Bromoacetic anhydride was added to an aqueous solution of triethylenetetramine and stirred to mix. Add nitrogen-containing organic complexing agent, sodium tripolyphosphate, hexamethylenetetramine and sodium thiosulfate, and stir to mix.
[0007] Preferably, a complexing agent is prepared by the following method: Add 16-22 parts of bromoacetic anhydride to 50-100 parts of triethylenetetramine aqueous solution and stir and mix at 40-50℃ for 1-3 hours; Add 15-25 parts of nitrogen-containing organic complexing agent, 15-25 parts of sodium tripolyphosphate, 8-18 parts of hexamethylenetetramine and 10-20 parts of sodium thiosulfate, and stir for 10-30 minutes. The triethylenetetramine aqueous solution contains 10-20 wt% triethylenetetramine. All parts mentioned above are by weight.
[0008] The nitrogen-containing organic complexing agent is one or more selected from 5-p-hydroxyphenylhydantoin, thioaminourea, cyanoacetylurea, 6-aminouracil, and 5-bromo-6-aminouracil. Preferably, the nitrogen-containing organic complexing agent is 5-p-hydroxyphenylhydantoin and / or 5-bromo-6-aminouracil.
[0009] The present invention also provides a metal complexing reducing agent, comprising the following raw materials: Complexing agent 15-45 wt%; Sodium dodecylbenzenesulfonate 1-6 wt% Cashew phenol polyoxyethylene ether 6-18 wt%; Octylphenol OP-10 2-10wt% Polyethylene glycol-800 1-2wt%; The remainder is water.
[0010] Preferably, a metal complexing reducing agent comprises the following raw materials: Complexing agent 20-40 wt%; Sodium dodecylbenzenesulfonate 1-4 wt% Cashew phenol polyoxyethylene ether 8-14 wt%; Octylphenol OP-10 4-8wt% Polyethylene glycol-800 1-2wt%; The remainder is water.
[0011] The present invention also provides a method for preparing a metal complexing reducing agent, comprising the following steps: mixing a complexing agent, sodium dodecylbenzenesulfonate, cashew phenol polyoxyethylene ether, octylphenol OP-10, polyethylene glycol-800 and water evenly.
[0012] The application of a metal complexing reducing agent in the hot-dip galvanizing process of steel parts includes the following steps: pickling the steel parts in a complexing pickling solution containing a metal complexing reducing agent and hydrochloric acid, then immersing them in an aqueous solution of ammonium chloride and / or zinc chloride, and finally sending them into a hot-dip galvanizing bath for hot-dip galvanizing.
[0013] Preferably, the application of a metal complexing reducing agent in the hot-dip galvanizing process of steel parts includes the following steps: (1) Pickling steel parts in a complexing pickling solution containing a metal complexing reducing agent and hydrochloric acid, wherein the complexing pickling solution contains 1-3 wt% metal complexing reducing agent and 8-16 wt% hydrochloric acid; (2) Then soak in a 6-11 wt% ammonium chloride and / or zinc chloride aqueous solution at 20-40°C; (3) The steel parts are sent into the hot-dip galvanizing tank for hot-dip galvanizing.
[0014] More preferably, the application of a metal complexing reducing agent in the hot-dip galvanizing process of steel parts includes the following steps: (1) Pickling the steel parts in a complex pickling solution containing a metal complex reducing agent and hydrochloric acid. The specific pickling steps are as follows: immerse the steel parts in the complex pickling solution at 20-40°C for 15-30 minutes. The complex pickling solution contains 1-3wt% metal complex reducing agent and 8-16wt% hydrochloric acid. The weight of the complex pickling solution is 20-50 times that of the steel parts. (2) Then immerse the steel parts in an aqueous solution of 6-11 wt% ammonium chloride and / or zinc chloride at 20-50 times their weight for 10-30 minutes at 20-40°C; (3) The steel parts are sent into the hot-dip galvanizing tank for hot-dip galvanizing.
[0015] In this invention, bromoacetic anhydride reacts with triethylenetetramine to form an amide compound. This is a typical amidation reaction, in which anhydride reacts with an amine to form an amide. The bromine atom may provide additional reactivity, contributing to the formation of complexing agents with specific chemical properties. Nitrogen-containing organic complexing agents enhance the metal complexing ability of the final product, improving selectivity and stability, by forming complexes with metal ions through their functional groups such as cyano, amino, and uracil rings. Sodium tripolyphosphate can improve stability and reduce metal ion deposition and corrosion. Hexamethylenetetramine improves metal treatment effects or acts as a corrosion inhibitor, while sodium thiosulfate is used to enhance complexing ability, prevent oxidation reactions, and improve the effectiveness of metal treatment.
[0016] The application of the metal complexing reducing agent of this invention in the hot-dip galvanizing process of steel parts not only ensures deep cleaning and uniform treatment of the steel surface, but also improves the overall quality and durability of the coating. By using the metal complexing reducing agent during the pickling process, this invention effectively removes the oxide layer and contaminants from the steel surface, while reducing chemical loss and corrosion of the steel, providing an ideal substrate for galvanizing. Furthermore, the precise control of the pretreatment steps, including the ammonium chloride and / or zinc chloride immersion process, further optimizes the steel surface, making the galvanized layer more uniform and robust. Overall, this treatment method not only enhances the adhesion of the galvanized layer, but also improves the uniformity and corrosion resistance of the coating, thereby significantly extending the service life of steel parts and improving their performance under various environmental conditions. Attached Figure Description
[0017] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0018] Figure 1 This is a graph showing the test data for copper sulfate titration time.
[0019] Figure 2 This is a graph showing the corrosion rate test data. Detailed Implementation
[0020] The invention will be more readily understood by referring to the following detailed description of preferred embodiments and included examples. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. In case of conflict, the definitions in this specification shall prevail.
[0021] A complexing agent is prepared by the following method: Add 16-22 parts of bromoacetic anhydride to 50-100 parts of triethylenetetramine aqueous solution and stir and mix at 40-50℃ for 1-3 hours; Add 15-25 parts of nitrogen-containing organic complexing agent, 15-25 parts of sodium tripolyphosphate, 8-18 parts of hexamethylenetetramine and 10-20 parts of sodium thiosulfate, and stir for 10-30 minutes.
[0022] The triethylenetetramine aqueous solution contains 10-20 wt% triethylenetetramine. All parts mentioned above are by weight.
[0023] The nitrogen-containing organic complexing agent is one or more selected from 5-p-hydroxyphenylhydantoin, thioaminourea, cyanoacetylurea, 6-aminouracil, and 5-bromo-6-aminouracil. Preferably, the nitrogen-containing organic complexing agent is 5-p-hydroxyphenylhydantoin and / or 5-bromo-6-aminouracil.
[0024] Bromoacetic anhydride, as a reactant, reacts with triethylenetetramine to form an amide compound. Its unique feature is the presence of a reactive bromine atom, which may endow the reaction product with special chemical properties, such as higher reactivity or stronger complexing ability. The presence of the bromine atom may allow the newly formed amide compound to undergo further chemical modification or participate in other types of chemical reactions.
[0025] As a polyamine compound, triethylenetetramine contains multiple amino groups that can form coordination bonds with metal ions. These amino groups, while reacting with bromoacetic anhydride to form amide bonds, also provide additional complexation sites. Therefore, triethylenetetramine not only participates in the synthesis of complexing agents, but its own amino groups also directly participate in the complexation with metal ions, enhancing the multifunctionality and efficiency of the complexing agents.
[0026] Nitrogen-containing organic complexing agents form complexes with metal ions through their unique functional groups. Their addition not only enhances the metal complexing ability of the complexing agent, but also improves the selectivity for specific metal ions and the overall stability of the complexing agent.
[0027] Sodium tripolyphosphate is commonly used in water treatment for softening water and preventing metal corrosion. In complexing agents, its addition may help reduce metal ion deposition and corrosion, thereby improving the stability and effectiveness of the complexing agent. Sodium tripolyphosphate can effectively inhibit oxidation and corrosion processes on metal surfaces by forming stable complexes with metal ions. Furthermore, it may improve the treatment effect of metal surfaces, such as increasing gloss or improving adhesion, making the metal surface more suitable for subsequent processing or applications.
[0028] The application of hexamethylenetetramine in complexing agents may be related to its chemical properties. The addition of hexamethylenetetramine may enhance the corrosion inhibition properties and metal treatment effects of the complexing agent, particularly in preventing metal surface corrosion and improving metal processing techniques. It may improve the surface properties and corrosion resistance of metals by forming a protective film on the metal surface or reacting with metal ions.
[0029] Sodium thiosulfate, a commonly used reducing agent, may play a role in complexing agents due to its reducing properties. Its addition can prevent oxidation reactions and enhance the stability and durability of the complexing agent. Furthermore, sodium thiosulfate may react with metal ions to improve metal treatment effects, such as reducing metal surface oxidation and increasing metal gloss.
[0030] In summary, the combination of these raw materials provides a versatile and highly efficient metal complexing agent suitable for a wide range of metal processing and chemical applications. Each component is added to enhance the overall performance of the complexing agent, including its complexing ability with metal ions, stability, corrosion inhibition, and treatment effectiveness.
[0031] A metal complex reducing agent, comprising the following raw materials: Complexing agent 20-40 wt%; Sodium dodecylbenzenesulfonate 1-4 wt% Cashew phenol polyoxyethylene ether 8-14 wt%; Octylphenol OP-10 4-8wt% Polyethylene glycol-800 1-2wt%; The remainder is water.
[0032] A method for preparing a metal complexing reducing agent includes the following steps: mixing a complexing agent, sodium dodecylbenzenesulfonate, cashew phenol polyoxyethylene ether, octylphenol OP-10, polyethylene glycol-800 and water evenly.
[0033] In the metal complexing reducing agent of this invention, the complexing agent is the main component, capable of forming stable complexes with metal ions. During metal processing, particularly in hot-dip galvanizing, the complexing agent reacts with ions (such as iron ions) on the metal surface to form stable complexes. This complex formation facilitates the removal of oxide layers and other corrosion products from the metal surface. In hot-dip galvanizing, the metal surface typically requires thorough cleaning to ensure coating quality. By reacting with ions on the metal surface, the complexing agent helps remove surface oxides and other contaminants, providing a cleaner and more active surface for galvanizing. Coating adhesion is a critical parameter during galvanizing. By forming stable complexes, the complexing agent can alter the chemical properties of the metal surface, enhancing the bond between the coating and the base metal. This enhanced adhesion ensures the uniformity and durability of the coating. In addition to enhancing adhesion, the complexing agent also contributes to achieving a uniform coating distribution. By removing uneven oxide layers from the metal surface, the complexing agent helps obtain a smoother, more consistent coating, which is crucial for maintaining the overall appearance and performance of the coating.
[0034] Sodium dodecylbenzenesulfonate, cashew phenol polyoxyethylene ether, octylphenol OP-10, and polyethylene glycol-800 also significantly influence the performance of metal complexing reducing agents. Sodium dodecylbenzenesulfonate is an anionic surfactant that reduces the surface tension of water, increases the wettability of liquids, and helps improve the cleaning effect on metal surfaces. Cashew phenol polyoxyethylene ether and octylphenol OP-10 are nonionic surfactants that further enhance the cleaning effect. Cashew phenol polyoxyethylene ether is a nonionic surfactant with cashew phenol (a derivative of phenol) as its lipophilic group, exhibiting good emulsifying, dispersing, and wetting properties. In its chemical structure, the cashew phenol moiety provides hydrophobicity, while the polyoxyethylene ether chain provides hydrophilicity. Octylphenol OP-10 is a nonionic surfactant with octylphenol as its lipophilic group. In its chemical structure, the octylphenol moiety provides hydrophobicity, while the polyoxyethylene ether chain provides hydrophilicity. In general, the main difference between these two compounds lies in their lipophilic moieties (cashew phenol and octylphenol), which affects their chemical properties and applications. Although they all contain polyoxyethylene ether chains, their uses and effects differ due to the different lipophilic groups. In this invention, they are used in combination for better results.
[0035] Polyethylene glycol-800 helps maintain the uniformity and stability of the solution by increasing its overall viscosity, which is particularly important for metal processing such as hot-dip galvanizing. Its molecular structure allows the solution to more effectively wet the metal surface, ensuring uniform coverage across the entire surface to be treated, thus improving the consistency of the treatment effect. Furthermore, the lubricating properties of polyethylene glycol-800 reduce friction during metal processing, helping to protect the integrity of the metal surface and improve treatment quality. In the formulation, polyethylene glycol-800 interacts with other components such as complexing agents and surfactants to enhance the overall effectiveness of the formulation, especially in cleaning and decontamination. Therefore, polyethylene glycol-800, in the metal complexing reducing agent of this invention, not only improves the effect of the metal processing but also ensures the uniformity and high quality of the process, making it an indispensable component of the hot-dip galvanizing process.
[0036] The application of a metal complexing reducing agent in the hot-dip galvanizing process of steel parts includes the following steps: (1) The steel parts are pickled in a complexing pickling solution containing a metal complexing reducing agent and hydrochloric acid. The specific pickling steps are as follows: the steel parts are immersed in the complexing pickling solution at 20-40°C for 15-30 minutes. The complexing pickling solution contains 1-3 wt% metal complexing reducing agent and 8-16 wt% hydrochloric acid. The weight of the complexing pickling solution is 20-50 times that of the steel parts. The main function of the complexing pickling solution is to remove the oxide layer (such as rust) and other dirt from the surface of the steel parts. If these oxide layers and dirt are not removed, they will seriously affect the quality and adhesion of the galvanized layer. Hydrochloric acid plays a key role in the complexing pickling solution. It dissolves these oxides and dirt through chemical reaction. The metal complexing reducing agent plays an important role in the pickling process. It not only helps to stabilize the metal ions in the complexing pickling solution and reduce further corrosion of the steel, but also improves the pickling efficiency. By forming complexes with metal ions, the complexing agent helps to remove the oxide layer and dirt on the surface more effectively.
[0037] (2) Then, the steel parts are immersed in an aqueous solution of 6-11 wt% ammonium chloride and / or zinc chloride at 20-50 times their weight at 20-40°C for 10-30 minutes. During the immersion process, the ammonium chloride and / or zinc chloride react with the steel surface to form a uniform salt film. This salt film is crucial for the subsequent hot-dip galvanizing because it helps zinc to better bond with the steel substrate. It not only helps to improve the adhesion of the galvanized layer but also enhances the uniformity and overall quality of the coating. In addition, the salt film can promote the uniform distribution of zinc on the steel surface, thereby avoiding uneven coating or coating defects during the hot-dip galvanizing process.
[0038] (3) The steel parts are placed in a hot-dip galvanizing bath for hot-dip galvanizing. This step is to form a protective zinc layer on the surface of the steel to improve its corrosion resistance.
[0039] In a specific embodiment of this invention, sodium dodecylbenzenesulfonate is sodium dodecylbenzenesulfonate powder LAS95 provided by Nanjing Milan New Materials Co., Ltd. Cashew phenol polyoxyethylene ether is BGF-7 industrial grade cashew phenol polyoxyethylene ether provided by Xingtai Xinlanxing Technology Co., Ltd. Octylphenol OP-10 is industrial grade emulsifier OP-10 octylphenol polyoxyethylene ether provided by Xingtai Xinlanxing Technology Co., Ltd. Polyethylene glycol-800 is polyethylene glycol PEG-800 provided by Jiangsu Haian Petrochemical Plant. Example 1:
[0040] One complexing pickling solution is an aqueous solution of 2 wt% metal complexing reducing agent and 12 wt% hydrochloric acid.
[0041] The metal complexing reducing agent comprises the following raw materials: 30 wt% complexing agent; 3 wt% sodium dodecylbenzenesulfonate; 10 wt% cashew phenol polyoxyethylene ether; 6 wt% octylphenol OP-10; 1.5 wt% polyethylene glycol-800; and the balance being water. The preparation method of the metal complexing reducing agent is as follows: the complexing agent, sodium dodecylbenzenesulfonate, cashew phenol polyoxyethylene ether, octylphenol OP-10, polyethylene glycol-800, and water are stirred and mixed evenly at 50°C, and then cooled to room temperature.
[0042] The complexing agent is prepared by the following method: 18 parts of bromoacetic anhydride were added to 80 parts of triethylenetetramine aqueous solution and stirred at 45°C for 2 hours. Add 20 parts of nitrogen-containing organic complexing agent 5-p-hydroxyphenylhydantoin, 20 parts of sodium tripolyphosphate, 12 parts of hexamethylenetetramine and 15 parts of sodium thiosulfate, and stir for 20 minutes.
[0043] The triethylenetetramine aqueous solution is an aqueous solution with a triethylenetetramine content of 15 wt%; All parts mentioned above are by weight. Example 2:
[0044] The difference from Example 1 is that the nitrogen-containing organic complexing agent in the complexing agent preparation method is 20 parts by mass of thioaminourea. Example 3:
[0045] The difference from Example 1 is that the nitrogen-containing organic complexing agent in the complexing agent preparation method is 20 parts by mass of cyanoacetylurea. Example 4:
[0046] The difference from Example 1 is that the nitrogen-containing organic complexing agent in the complexing agent preparation method is 20 parts by mass of 5-bromo-6-aminouracil. Example 5:
[0047] The difference from Example 1 is that the nitrogen-containing organic complexing agent in the complexing agent preparation method is 10 parts by weight of 5-p-hydroxyphenylhydantoin and 10 parts by weight of 5-bromo-6-aminouracil.
[0048] Comparative Example 1:
[0049] The difference from Example 1 is that the complexing agent is prepared by the following method: 18 parts of bromoacetic anhydride were added to 80 parts of diethylenetriamine aqueous solution and stirred at 45°C for 2 hours. Add 20 parts of nitrogen-containing organic complexing agent 5-p-hydroxyphenylhydantoin, 20 parts of sodium tripolyphosphate, 12 parts of hexamethylenetetramine and 15 parts of sodium thiosulfate, and stir for 20 minutes.
[0050] The diethylenetriamine aqueous solution is an aqueous solution with a diethylenetriamine content of 15 wt%. All parts mentioned above are by weight.
[0051] Comparative Example 2:
[0052] The difference from Example 1 is that the complexing agent is prepared by the following method: 18 parts of bromoacetic anhydride were added to 80 parts of n-butylamine aqueous solution and stirred at 45°C for 2 hours. Add 20 parts of nitrogen-containing organic complexing agent 5-p-hydroxyphenylhydantoin, 20 parts of sodium tripolyphosphate, 12 parts of hexamethylenetetramine and 15 parts of sodium thiosulfate, and stir for 20 minutes.
[0053] The n-butylamine aqueous solution is an aqueous solution with a n-butylamine content of 15 wt%; All parts mentioned above are by weight.
[0054] Comparative Example 3:
[0055] The difference from Example 1 is that the complexing agent is prepared by the following method: 18 parts of maleic anhydride were added to 80 parts of triethylenetetramine aqueous solution and stirred at 45°C for 2 hours. Add 20 parts of nitrogen-containing organic complexing agent 5-p-hydroxyphenylhydantoin, 20 parts of sodium tripolyphosphate, 12 parts of hexamethylenetetramine and 15 parts of sodium thiosulfate, and stir for 20 minutes.
[0056] The triethylenetetramine aqueous solution is an aqueous solution with a triethylenetetramine content of 15 wt%; All parts mentioned above are by weight.
[0057] Blank example:
[0058] One complexing pickling solution is an aqueous solution of 12wt% hydrochloric acid.
[0059] Test Example 1:
[0060] Steel parts (50cm×50cm×2cm) were pickled in the complex pickling solutions of Examples 1-5, Comparative Examples 1-3 and Blank Examples, respectively. The specific pickling steps were as follows: the steel parts were immersed in the complex pickling solution at 30°C for 20 minutes and then dried at 90°C. The weight of the complex pickling solution was 40 times that of the steel parts.
[0061] A copper sulfate drop solution was prepared by mixing 40 ml of a 0.3 mol / L copper sulfate solution (CuSO4·5H2O), 20 ml of a 10% NaCl solution, and 2 ml of a 0.2 mol / L HCl solution.
[0062] Two drops of copper sulfate solution were applied to the steel parts after the hot-dip galvanizing process described above. A stopwatch was started, and the time it took for the solution to change from sky blue to reddish-brown was recorded as the copper sulfate titration time (s). Specific data are shown in Table 1. The detailed test data were plotted... Figure 1 .
[0063] The extended titration time of copper sulfate reflects an enhanced antioxidant capacity of the steel parts, meaning they can be left in air for longer periods without oxidation. This finding is significant for addressing the need for rapid hot-dip galvanizing of steel parts after hydrochloric acid pickling to prevent oxidation, effectively improving the flexibility and efficiency of industrial production processes.
[0064] Table 1: Test Table for Copper Sulfate Titration Time
[0065] Among the nitrogen-containing organic complexing agents in Comparative Examples 1-4, 5-bromo-6-aminouracil exhibited superior performance in Example 4. From a chemical perspective, the excellent performance of 5-bromo-6-aminouracil in Example 4 can be attributed to its unique molecular structure and chemical properties. The uracil ring of this compound is a nitrogen-containing heterocyclic structure, naturally possessing the ability to form complexes with metal ions. When bromine atoms are introduced, their larger atomic radius and higher electronegativity increase the overall polarity and electron density of the molecule, which may further enhance its complexing ability with metal ions. This strong complexing ability helps form a more stable protective layer on the steel surface, thereby improving the oxidation resistance of steel parts in air. This improved oxidation resistance is reflected in the extended copper sulfate titration time, indicating that compared to other compounds, 5-bromo-6-aminouracil is more effective in preventing surface oxidation and improving the stability and adaptability of the material in subsequent processing.
[0066] Furthermore, the combination of 5-p-hydroxyphenylhydantoin and 5-bromo-6-aminouracil in Example 5 exhibited a significant synergistic effect. 5-p-hydroxyphenylhydantoin forms a stable complex with metal ions due to its unique functional group, while 5-bromo-6-aminouracil increases the complexation sites with metal ions through the additional amino group in the uracil ring. The introduction of the bromine atom further enhances the molecular polarity and electron density, strengthening the complexation with metal ions. This combination enhances the diversity and functionality of the complexing agent, promotes the formation of a more robust protective layer on the steel surface, and improves antioxidant properties, manifested in a significant extension of the copper sulfate titration time.
[0067] In Example 1, the use of triethylenetetramine was more effective than that of diethylenetriamine and n-butylamine in Comparative Examples 1 and 2, respectively, primarily due to the molecular structure and functionality of triethylenetetramine. Triethylenetetramine has more amino groups, providing more active sites and thus forming more stable complexes with metal ions. This stable complexation helps form a more effective protective layer on the steel surface, enhancing its oxidation resistance and corrosion resistance. In contrast, diethylenetriamine and n-butylamine, due to their simpler molecular structures and fewer active sites, have relatively weaker complexing abilities, resulting in less significant protective effects compared to triethylenetetramine.
[0068] Test Example 2:
[0069] Using 45# steel test pieces (45×15×1 mm, with 50% rust on the surface), the test pieces were first degreased, then thoroughly cleaned with deionized water and dried, followed by weighing. The cleaned test pieces were then immersed in a complexing pickling solution at 30°C for 20 minutes, with the solution volume being 50 times the weight of the test piece. After pickling, the test pieces were rinsed again with deionized water, dried, and weighed to evaluate the pickling effect. Finally, the corrosion rate was calculated. Specific test data were plotted... Figure 2 .
[0070] Corrosion rate = (initial test piece - mass of test piece after pickling) ÷ time to completely remove rust.
[0071] Table 2: Corrosion Rate Test Table
[0072] The complexing agents used in Examples 1-4 (such as 5-p-hydroxyphenylhydantoin, thioaminourea, cyanoacetylurea, and 5-bromo-6-aminouracil) exhibit excellent metal complexing capabilities. These complexing agents effectively reduce the corrosion rate during pickling by forming stable complexes with metal ions on the steel surface. In particular, 5-bromo-6-aminouracil, due to its structural characteristics, exhibits a superior complexing effect, resulting in a lower corrosion rate. In the blank example, no complexing agent was used; only hydrochloric acid was used for pickling. In this case, due to the lack of protective effects from the complexing agent, the steel specimens experienced a faster corrosion rate during pickling, leading to a higher corrosion rate.
[0073] The copper sulfate titration time test in Test Example 1 was used to evaluate the oxidation resistance of the steel part's surface. A longer copper sulfate titration time indicates better oxidation resistance of the steel part's surface, allowing it to resist oxidation from the air for a longer period. The corrosion rate test in Test Example 2 focused on the quality changes of the steel part during pickling, measuring the intensity of the pickling solution's corrosive effect on the steel part. A slower corrosion rate indicates a weaker corrosive effect of the pickling solution on the steel part, and less damage to the metal. The different trends in the results of the two tests reflect the performance of the steel part in different chemical processes, which is closely related to the chemical structure and mechanism of action of the complexing agent used. The excellent performance in Example 4 demonstrates the effectiveness of its complexing agent in improving the oxidation resistance of the steel part and slowing down the corrosion rate.
[0074] Application example:
[0075] The application of a metal complexing reducing agent in the hot-dip galvanizing process of steel parts includes the following steps: (1) The steel parts (50cm×50cm×2cm) were pickled in the complex pickling solutions prepared in Examples 1-5 and Comparative Examples 1-3 respectively. The specific pickling steps were as follows: the steel parts were immersed in the complex pickling solution at 30°C for 20 minutes. The weight of the complex pickling solution was 40 times that of the steel parts. (2) Then immerse the steel parts in an 8wt% ammonium chloride aqueous solution at 30°C for 20 minutes, which is 40 times their weight. (3) The steel parts are immersed in molten zinc in a hot-dip galvanizing bath at 450°C for 60 seconds. After removal, they are allowed to cool naturally to room temperature.
[0076] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions conceived without inventive effort should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.
Claims
1. A complexing agent, characterized by, It is prepared by the following method: Add 16-22 parts of bromoacetic anhydride to 50-100 parts of triethylenetetramine aqueous solution and stir and mix at 40-50℃ for 1-3 hours; Add 15-25 parts of nitrogen-containing organic complexing agent, 15-25 parts of sodium tripolyphosphate, 8-18 parts of hexamethylenetetramine and 10-20 parts of sodium thiosulfate, and stir for 10-30 minutes. The triethylenetetramine aqueous solution contains 10-20 wt% triethylenetetramine. All parts mentioned above are by weight.
2. The complexing agent according to claim 1, characterized in that, The nitrogen-containing organic complexing agent is one or more of 5-p-hydroxyphenylhydantoin, thioaminourea, cyanoacetylurea, 6-aminouracil, and 5-bromo-6-aminouracil.
3. The complexing agent according to claim 2, characterized in that, The nitrogen-containing organic complexing agent is 5-p-hydroxyphenylhydantoin and / or 5-bromo-6-aminouracil.
4. A metal complexing reducing agent, characterized in that, Including the following raw materials: The complexing agent according to any one of claims 1-3 is 15-45 wt%; Sodium dodecylbenzenesulfonate 1-6 wt% Cashew phenol polyoxyethylene ether 6-18 wt%; Octylphenol OP-10 2-10wt% Polyethylene glycol-800 1-2wt%; The remainder is water.
5. The metal complex reducing agent according to claim 4, characterized in that, Including the following raw materials: The complexing agent according to any one of claims 1-3 is 20-40 wt%; Sodium dodecylbenzenesulfonate 1-4 wt% Cashew phenol polyoxyethylene ether 8-14 wt%; Octylphenol OP-10 4-8wt% Polyethylene glycol-800 1-2wt%; The remainder is water.
6. The method for preparing the metal complex reducing agent according to claim 4 or 5, characterized in that, The process includes the following steps: mixing the complexing agent, sodium dodecylbenzenesulfonate, cashew phenol polyoxyethylene ether, octylphenol OP-10, polyethylene glycol-800 and water until homogeneous.
7. The application of the metal complexing reducing agent according to claim 4 or 5 in the hot-dip galvanizing process of steel parts, characterized in that, The process includes the following steps: pickling the steel parts in a complexing pickling solution containing a metal complexing reducing agent and hydrochloric acid, then immersing them in an aqueous solution of ammonium chloride and / or zinc chloride, and finally sending them into a hot-dip galvanizing bath for hot-dip galvanizing.
8. The application of the metal complexing reducing agent according to claim 7 in the hot-dip galvanizing process of steel parts, characterized in that, Includes the following steps: (1) Pickling steel parts in a complexing pickling solution containing a metal complexing reducing agent and hydrochloric acid, wherein the complexing pickling solution contains 1-3 wt% metal complexing reducing agent and 8-16 wt% hydrochloric acid; (2) Then soak in a 6-11 wt% ammonium chloride and / or zinc chloride aqueous solution at 20-40°C; (3) The steel parts are sent into the hot-dip galvanizing tank for hot-dip galvanizing.
9. The application of the metal complexing reducing agent according to claim 8 in the hot-dip galvanizing process of steel parts, characterized in that, Includes the following steps: (1) Pickling the steel parts in a complex pickling solution containing a metal complex reducing agent and hydrochloric acid. The specific pickling steps are as follows: immerse the steel parts in the complex pickling solution at 20-40°C for 15-30 minutes. The complex pickling solution contains 1-3wt% metal complex reducing agent and 8-16wt% hydrochloric acid. The weight of the complex pickling solution is 20-50 times that of the steel parts. (2) Then immerse the steel parts in an aqueous solution of 6-11 wt% ammonium chloride and / or zinc chloride at 20-50 times their weight for 10-30 minutes at 20-40°C; (3) The steel parts are sent into the hot-dip galvanizing tank for hot-dip galvanizing.
Citation Information
Patent Citations
Composite corrosion and scale inhibition fungicide and preparation method thereof
CN108056107A
Hot dip galvanizing process of corrosion-resistant steel pipe
CN111304572A