A production method for avoiding defects of medium and high carbon steel flat coils based on CSP process

By optimizing the heating, descaling, rolling, cooling, and coiling parameters in the CSP process, the problem of flattening defects after coiling of medium and high carbon steel was solved, achieving high-quality and efficient hot-rolled strip steel production.

CN118268392BActive Publication Date: 2026-11-24GANSU JIU STEEL GRP HONGXING IRON & STEEL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410579742.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-11
Publication Date
2026-11-24
Estimated Expiration
2044-05-11

AI Technical Summary

Technical Problem

Hot-rolled medium and high carbon steel coils are prone to flattening defects after coiling, which prevents the mandrel from entering the core when uncoiling, resulting in cutting waste and reduced production efficiency.

Method used

By optimizing the CSP process, including controlling parameters such as slab heating time and temperature, descaling pressure, rolling reduction rate, laminar cooling mode, coiling tension and temperature, coiler speed and interlayer coefficient, the steel coil is ensured to be coiled in the austenitic region and tension is increased, thus avoiding volume expansion caused by phase transformation.

Benefits of technology

This effectively avoids flattening defects, reduces cutting losses and labor costs, and improves the quality and production efficiency of hot-rolled strip steel products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118268392B_ABST
    Figure CN118268392B_ABST
Patent Text Reader

Abstract

This invention discloses a production method based on the CSP process to avoid the flat coil defect of medium and high carbon steel. By controlling the coiling tension and coiling temperature, the method solves the problem of coil collapse defect after coiling of medium and high carbon steel, effectively avoiding the cutting damage and labor costs caused by cutting off the inner circle of the collapsed coil, and improving the product quality and labor productivity of hot-rolled strip steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of hot-rolled strip steel rolling, and specifically relates to a method for improving the coil shape quality of hot-rolled high-carbon steel. Background Technology

[0002] CSP (Compact Slab Continuous Casting and Rolling) technology, also known as compact hot-rolled strip steel production technology, is the world's earliest industrialized thin slab continuous casting and rolling technology. It involves directly feeding high-temperature, defect-free slabs produced by a continuous casting machine into a roller-hearth tunnel furnace for brief homogenization and holding, followed by direct rolling into hot-rolled strip. The roller-hearth furnace connects the continuous casting and rolling processes to form a continuous casting and rolling production line. Compared to the traditional continuous casting-cooling-cleaning-heating-rolling process, continuous casting and rolling offers advantages such as shorter production cycles, lower fixed asset investment, higher metal yield, better steel properties, and lower energy consumption.

[0003] Hot-rolled medium-high carbon steel strip is widely used in the machinery and tool manufacturing industries. It typically refers to steel products with a carbon content of 0.25% to 1.25% by mass, possessing high hardness, high toughness, and good wear resistance. Major grades include S35C, 45, 45AE, S50C, 50AE, 50AM, 60, 65Mn, 40Mn, 45Mn, and 60Si2Mn.

[0004] Hot-rolled medium and high carbon steel slabs are heated and held in a heating furnace, rolled by a 6-stand continuous rolling mill, cooled by a laminar flow cooling system, rolled into steel coils by a coiler, and then air-cooled to room temperature in a warehouse before being shipped.

[0005] After hot-rolled high-carbon steel strip is coiled, it undergoes a phase transformation from austenite to ferrite, resulting in volume expansion and gaps between coil layers. Under its own weight, the coil flattens (becomes elliptical), especially in thin strips with a thickness ≤3.5mm, where the flattening defect is more severe. Because the core of the flattened coil is elliptical, and the minimum inner diameter of the elliptical core is smaller than the outer diameter of the uncoiler mandrel, the mandrel cannot enter the core during uncoiling, preventing normal uncoiling. To uncoil the flattened coil, 5-20 turns of the core must be manually removed (depending on the coil thickness and flattening condition), making the minimum radius of the ellipse larger than the outer diameter of the uncoiler mandrel. This results in wasted steel coil material, increased labor costs, and reduced production efficiency. Summary of the Invention

[0006] The purpose of this invention is to provide a production method based on CSP process to avoid defects in medium and high carbon steel flat coils, thereby solving the quality defect problem of medium and high carbon steel flat coils.

[0007] To achieve the above objectives, the present invention adopts the following technical solution: A production method for avoiding defects in medium and high carbon steel flat coils based on the CSP process includes the following steps: A. Medium and high carbon steel slabs produced by thin slab continuous casting machines have a thickness of 70~60mm. The slabs are directly fed into a roller bottom tunnel heating furnace. The heating time in the furnace is controlled at 15~30min, and the furnace exit temperature is controlled at 1150~1190℃.

[0008] B. The slab exits the furnace and passes through two high-pressure water descaling processes at a speed of 0.3~0.5m / s. The descaling pressure in the front manifold is 200~240bar, and the descaling pressure in the rear manifold is 300~360bar. The iron oxide scale on the surface of the slab is removed by high-pressure water descaling.

[0009] C. The descaled slab is rolled using a 6-stand continuous rolling process. The reduction rate for each stand is controlled as follows: F1: 55%~65%, F2: 45~55%, F3: 40~48%, F4: 30~35%, F5: 20~30%, F6: 15~20%. The final rolling temperature is controlled at 900~940℃. The rolling speed is automatically set by a secondary system to ensure the final rolling temperature.

[0010] D. After rolling, the strip undergoes laminar flow cooling to reduce its temperature from the final rolling temperature to the coiling temperature. For medium- and high-carbon strips, the laminar cooling mode is selected as front-stage dispersed cooling, with cooling water turned on in the front stage and air cooling turned off in the rear stage. The laminar cooling rate is controlled below 25℃ / s.

[0011] E. After the strip is cooled in layers, it is coiled using an underground coiler to improve the lead rate when coiling the strip head. The speed of the coiler pinch roll is 109% of the strip speed, the speed of the coiler auxiliary roll is 115% of the strip speed, and the speed of the coiler mandrel is 113% of the strip speed.

[0012] F. Increase the winding tension of the belt. The automatic winding tension setting for medium and high carbon steel at level two is 15~20 N / mm. 2 (Based on the change in strip thickness, the smaller the strip thickness, the greater the tension); the actual coiling tension of the strip is equal to the secondary set tension value plus the tension bonus.

[0013] (1) When the strip head enters the coiler to the tension establishment stage (belonging to the strip threading and tension establishment stage), the coiling tension setting value is 85% of the secondary setting coiling tension value. The tension additional value in this stage is 0.

[0014] (2) After the strip head enters the coiler for 20 meters (after tensioning), it enters the stable coiling stage. The tension increment is increased by stepwise, with an increase of 8 N / mm for every 10 meters. 2 The tension increment increased four times, successively: 0 N / mm 2 →8N / mm 2 →16N / mm2 →24N / mm 2 →32N / mm 2 The actual maximum winding tension can reach 52 N / mm. 2 .

[0015] (3) Maintain maximum tension during subsequent winding. By increasing the tension of the winding machine, the tightness between layers is improved, effectively resisting the degree of loosening.

[0016] (4) When the strip is coiled to a distance of 180 meters from the tail of the strip (which is the strip body stage), the additional coiling tension gradually decreases. The additional tension is reduced in four steps, starting from 32 N / mm. 2 →24N / mm 2 →16N / mm 2 →8N / mm 2 →0N / mm 2 .

[0017] (5) When the tail of the strip is 100 meters away from the pinch roll, the winding tension is 75% of the secondary set value and continues until the strip winding ends. The additional tension value during this stage is 0.

[0018] G. Adjust the interlayer coefficient of the strip steel during winding from 1.0 to 0.8, so that the calculated coil diameter is smaller than the actual coil diameter, which increases the tension during the winding process, making the layers of the steel coil fit tightly together, and the steel coil forms a rigid whole, making it less likely to flatten.

[0019] H. High-temperature coiling is adopted, with the coiling temperature set at the temperature at which medium-to-high carbon austenite begins to transform into ferrite (Ar3 temperature) +10℃~30℃. Generally, it is controlled between 720~760℃ (the higher the carbon content, the higher the coiling temperature). High-temperature coiling ensures that the steel coil remains entirely in the austenitic region during the coiling process, avoiding coiling in the two-phase region. This prevents premature phase transformation due to localized low strip temperatures, which can lead to uneven volume expansion and loose coiling. The coiling temperature of the first 10 meters of strip should be 0~20℃ higher than the strip body. The strip head is the end of the strip during rolling, resulting in rapid heat dissipation and a faster temperature drop compared to the strip body. Normally, the strip head temperature is more than 20℃ lower than the strip body temperature. Increasing the coiling temperature at the strip head aims to improve the overall temperature uniformity of the strip, preventing premature uneven phase transformation and uneven volume expansion at the head, which can cause loose coiling in the first few turns.

[0020] I. After winding, the steel coil waits on the winding machine core shaft for 10-20 seconds before being unwound to facilitate coil shaping.

[0021] J. After the steel coils are put into the warehouse, they should be stacked in a single layer or placed on the top layer to avoid squeezing between the steel coils and causing them to flatten.

[0022] Furthermore, in step A, a longer soaking time (15~30 min) and a higher furnace exit temperature (1150~1190℃) can effectively improve the uniformity of columnar crystal and austenite structure in the slab, reduce the difference between the head and tail and the middle of the slab, and reduce the performance difference between the two sides and the middle of the slab, thus laying the foundation for the uniformity of the microstructure and properties after rolling.

[0023] Furthermore, in step B, the two-pass high-pressure water descaling can effectively remove the iron oxide scale from the slab surface, avoiding the defect of iron oxide scale being pressed into the strip surface.

[0024] Furthermore, in step D, the medium-high carbon layer cooling mode is selected as front-end dispersed cooling. Dispersed cooling avoids the concentration of cooling water and avoids excessively low local temperature drops. The rear-end air cooling makes the strip coiling temperature more uniform, making the strip temperature more uniform during layer cooling and avoiding premature uneven phase transformation due to excessively low local temperatures.

[0025] Furthermore, in step E, increasing the lead rate during strip head winding allows the pinch rolls, auxiliary winding rolls, and mandrel to accelerate, increasing the acceleration of the strip head entering the coiler and ensuring that the strip head is tightly wound.

[0026] Furthermore, in step F, the winding tension is increased. Higher tension overcomes the deformation resistance of medium- and high-carbon steel, ensuring a tight coil and effectively preventing flattening. However, excessive tension can cause overcurrent tripping of the coiler's core shaft, and the tail of the coil may rebound at the moment of tail ejection on the last stand, easily leading to folding and buckling before the coiler's pinch rolls. Therefore, a two-stage tension setting with an additional tension value is adopted. This automatically achieves low tension at the beginning, gradually increasing tension in stages along the body, maintaining a stable high tension along the body, gradually decreasing tension near the tail, and finally achieving minimum tension at the tail. Tension is increased or decreased in stages every 10 meters to ensure smooth tension changes and prevent tension fluctuations from affecting the coil shape.

[0027] Furthermore, in step G, the interlayer coefficient of the strip steel during winding is adjusted from 1.0 to 0.8, so that the calculated coil diameter is smaller than the actual coil diameter, which increases the tension during the winding process, making the layers of the steel coil fit together tightly, and the steel coil forms a rigid whole, making it less likely to flatten.

[0028] Furthermore, in step H, the coiling temperature is controlled 10°C to 30°C above the temperature at which medium-high carbon austenite begins to transform into ferrite (Ar3 temperature). High-temperature coiling, between 720°C and 760°C, is adopted, significantly higher than the phase transformation initiation temperature of medium-high carbon steel. This avoids phase transformation during the layer cooling and coiling process, prevents premature phase transformation of localized austenite due to internal temperature differences in medium-high carbon steel, and avoids uneven expansion of the strip volume caused by localized austenite-to-ferrite phase transformation, thereby reducing the flattening of the coil due to interlayer friction. Simultaneously, high-temperature coiling contributes to the uniformity of the strip's mechanical properties, reduces the strength of medium-high carbon steel strip, and creates conditions for stable cold rolling and subsequent rolling processes.

[0029] The beneficial effects of this invention are: it provides a method for producing medium and high carbon strip steel, which solves the problem of coil collapse defect after coiling of medium and high carbon steel, effectively avoids the cutting damage and labor costs caused by cutting off the inner circle of the coil collapse defect, and improves the product quality and labor productivity of hot-rolled strip steel. Attached Figure Description

[0030] Figure 1 This is a schematic diagram illustrating the additional coiling tension during the production of 65Mn*1270*2.3mm strip steel according to an embodiment of the present invention.

[0031] Figure 2 This is a comparison chart showing the effects of not using (left) and using the method of the present invention (right) in the production of 65Mn*1270*2.3mm strip steel according to the present invention. Detailed Implementation

[0032] Taking the production of 65Mn*1270*2.3mm strip steel as an example.

[0033] A. The slab thickness produced by the thin slab continuous casting machine is 60mm, the heating time in the soaking furnace is 20min, the furnace exit temperature is 1180℃, and the final rolling temperature is 920℃.

[0034] B. The slab exits the furnace and passes through two high-pressure water descaling processes at a speed of 0.3~0.5m / s. The descaling pressure in the front manifold is 220bar, and the descaling pressure in the rear manifold is 350bar. The iron oxide scale on the surface of the slab is removed by high-pressure water descaling.

[0035] C. The descaled slabs are rolled using a 6-stand continuous rolling process, with the following reduction rates controlled for each stand: F1: 63.2%, F2: 53.8%, F3: 46.8%, F4: 34.2%, F5: 25.2%, F6: 19.3%.

[0036] D. After rolling, the strip undergoes laminar flow cooling, reducing its temperature from the final rolling temperature of 920℃ to the coiling temperature of 745℃. For medium-high carbon strips, the laminar cooling mode is selected as front-stage dispersed cooling, with cooling water opened in the front stage and air cooling in the rear stage. The strip speed is 8.3 m / s, and the laminar cooling rate is 20℃ / s.

[0037] E. Increase the lead rate during strip head winding and tensioning, with the pinch roll speed at 109% of the strip speed, the auxiliary winding roll speed at 115% of the strip speed, and the winding machine core shaft speed at 113% of the strip speed.

[0038] F. Increase the winding tension; the secondary winding tension is set to 20 N / mm. 2 The coiling tension at the head of the strip is 17 N / mm. 2 After winding 20 meters, the winding tension increases to 28 N / mm. 2 After winding 30 meters, the winding tension increases to 36 N / mm. 2 After winding 40 meters, the winding tension increases to 44 N / mm. 2 After winding 50 meters, the winding tension increases to 52 N / mm. 2 The winding tension is then maintained at 52 N / mm. 2 When the winding reaches a distance of 180 meters from the belt tail entering the pinch roller, the winding tension decreases from 52 N / mm. 2 Reduced to 44 N / mm 2 When the belt tail is 170 meters from the pinch roller, the winding tension decreases to 36 N / mm. 2 When the belt tail is 160 meters from the pinch roller, the winding tension decreases to 28 N / mm. 2 When the belt tail is 150 meters from the pinch roller, the winding tension decreases to 20 N / mm. 2 When the tail of the strip leaves the roll gap of the F3 mill (at which point the strip tail is approximately 100 meters from the pinch rolls), the coiling tension decreases to 15 N / mm. 2 This continues until the winding process ends.

[0039] G. Adjust the interlayer coefficient of the strip during coiling to 0.8.

[0040] H. High-temperature coiling is adopted. The theoretical temperature at which the austenite of 65Mn begins to transform into ferrite is 730℃. The coiling temperature is controlled between 740-750℃, and the coiling temperature of the first 10 meters of strip is 760℃.

[0041] I. After winding is completed, the steel coil waits on the mandrel in the winding machine for 15 seconds before being unwound.

[0042] J. After the steel coils are put into the warehouse, they are stacked in a single layer.

[0043] The result is, for example Figure 2As shown, the left side represents a flattened steel coil without the method of the present invention, and the right side represents a flattened steel coil without the defects after the method of the present invention is applied.

Claims

1. A production method for avoiding defects in medium and high carbon steel flat coils based on the CSP process, characterized in that, Includes the following steps: A. Medium and high carbon steel slabs produced by thin slab continuous casting machines have a thickness of 70~60mm. The slabs are directly fed into the roller bottom tunnel heating furnace. The heating time in the heating furnace is controlled at 15~30min, and the furnace exit temperature is controlled at 1150~1190℃. B. The slab exits the furnace and passes through two high-pressure water descaling processes at a speed of 0.3~0.5m / s. The descaling pressure in the front manifold is 200~240bar, and the descaling pressure in the rear manifold is 300~360bar. The iron oxide scale on the surface of the slab is removed by high-pressure water descaling. C. The descaled slab is rolled using a 6-stand continuous rolling process, with the following reduction rates controlled for each stand: F1: 55%~65%, F2: 45~55%, F3: 40~48%, F4: 30~35%, F5: 20~30%, F6: 15~20%; the final rolling temperature is controlled at 900~940℃; the rolling speed is automatically set by the secondary system to ensure the final rolling temperature. D. After rolling, the strip steel is cooled by laminar flow to reduce the strip steel temperature from the final rolling temperature to the coiling temperature; the medium and high carbon laminar cooling mode is selected as front-stage dispersed cooling, with the front-stage dispersed cooling water turned on and the rear-stage water-air cooling turned off, and the laminar cooling rate is controlled below 25℃ / s. E. After laminar cooling, the strip steel is coiled using an underground coiler. The coiler's pinch roll speed is 109% of the strip steel speed, the coiler's auxiliary coil roll speed is 115% of the strip steel speed, and the coiler's mandrel speed is 113% of the strip steel speed. F, increase the strip body winding tension; high carbon steel two set winding tension value is 15~20N / mm 2 , the actual winding tension of the strip is equal to the second set tension value plus the tension additional value; (1) The strip head enters the coiler to the tension establishment stage, that is, the strip threading and tension establishment stage; the coiling tension setting value is 85% of the secondary setting coiling tension value, and the tension additional value in this stage is 0; (2) After the strip head enters the coiler by 20 meters, it belongs to the stable coiling stage of the strip body; the tension additional value is increased by a stepwise increment method, and the tension additional value is increased by 8 N / mm every 10 meters 2 ; the tension additional value is increased 4 times, and the values are as follows: 0 N / mm 2 → 8 N / mm 2 → 16 N / mm 2 → 24 N / mm 2 → 32 N / mm 2 ; (3) When the strip is coiled to a distance of 180 meters from the tail of the strip, the additional coiling tension gradually decreases. The additional tension is reduced in four steps, starting from 32 N / mm. 2 →24N / mm 2 →16N / mm 2 →8N / mm 2 →0N / mm 2 ; (4) When the tail of the strip is 100 meters away from the pinch roll, the winding tension is 75% of the secondary set value and continues until the strip winding ends. The additional tension value during this stage is 0. G. Adjust the interlayer coefficient of the strip during coiling from 1.0 to 0.8; H. High-temperature winding is adopted, and the winding temperature is controlled between 720 and 760°C. At the same time, the winding temperature of the first 10 meters of strip steel should be 0 to 20°C higher than that of the strip body. I. After winding is completed, the steel coil should be left on the winding machine core shaft for 10-20 seconds before being unwound to facilitate the shaping of the steel coil; J. After the steel coils are put into the warehouse, they should be stacked in a single layer or placed on the top layer to avoid squeezing between the steel coils and causing them to flatten.

Citation Information

Patent Citations

  • Method of preventing steel coil tensile steel for hot rolled strip

    CN106825062A

  • Hot-rolled and thin low-alloy steel strip for 520 Mpa photovoltaic supoprt and CSP (cast steel plate) process production method of hot-rolled and thin low-alloy steel strip

    CN110144525A

  • Thin-gauge medium-high carbon steel type seasonal flat coil control method