T-shaped GH4169 high-temperature alloy rudder shaft forging processing method
By using an integrated forging method combining extrusion and upsetting, combined with numerical simulation and heat treatment, the problems of uneven grain size and low material utilization in T-shaped GH4169 high-temperature alloy rudder shafts were solved, achieving efficient production and high impact toughness forgings.
Patent Information
- Application Number
- CN202211729438.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-31
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-12-31
AI Technical Summary
Existing technologies make it difficult to effectively manufacture T-shaped GH4169 high-temperature alloy rudder shafts, resulting in uneven grain distribution, low material utilization, low processing efficiency, and difficulty in meeting the requirements for high impact toughness.
The forging method of extrusion and upsetting is adopted. The forging process is optimized by combining Deform numerical simulation software. The mold is designed and a screw press is used to control the heating temperature and strain. One-shot forming is carried out, followed by solution treatment and aging heat treatment, and finally surface cleaning.
It achieves uniform grain distribution in forgings, improves material utilization and processing efficiency, enhances room temperature impact performance, meets high impact toughness requirements, and is suitable for industrial production.
Smart Images

Figure CN118268488B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of forging technology, specifically to a method for processing T-shaped GH4169 high-temperature alloy rudder shaft forgings. Background Technology
[0002] As spacecraft continue to advance towards hypersonic speeds and longer endurance, their propulsion components must withstand higher temperatures and more demanding airflow environments. This places higher demands on the performance of various components, with the rudder shaft being a particularly critical part, requiring not only high strength but also greater impact toughness. The rudder shaft is made of GH4169 material to withstand high temperatures and airflow impacts, and its structure is as follows... Figure 1 , Figure 2 As shown, it includes a large end section 100 at the upper end and a columnar rod section 200 at the lower end. The top surface of the large end section 100 is a flat part, and the cross-section of the large end section 100 is a quadrilateral with rounded corners on all four sides. At the same time, it has positioning structures 300 that bulge outward to form arc-shaped curved surfaces on its opposite sides.
[0003] Because the rudder shaft is a T-shaped irregular part, both conformal forging and free forging are difficult to avoid the critical deformation of the GH4169 alloy, resulting in uneven grain distribution, insufficient room temperature impact toughness, or even substandard performance. These issues pose a threat to the stability and reliability of the part. Therefore, the mainstream process for producing rudder shaft parts currently involves machining from forged round bars or forged square billets. However, this process suffers from low material utilization and low processing efficiency. Summary of the Invention
[0004] To address the aforementioned problems, this invention provides a method for processing T-shaped GH4169 high-temperature alloy rudder shaft forgings. This method can be used to manufacture T-shaped GH4169 rudder shaft forgings, resulting in forgings with uniform grain distribution, while also achieving effective material utilization and high processing efficiency.
[0005] The technical solution is as follows: A method for processing a T-shaped GH4169 high-temperature alloy rudder shaft forging, characterized by the following steps: 1. Designing the forging; The T-shaped GH4169 rudder shaft forging includes a large end section at the upper end and a columnar rod section at the lower end. The top surface of the large end section is flat, and the cross-section of the large end section is a quadrilateral with rounded corners on all four sides. Simultaneously, its opposite sides in the length direction have outwardly protruding positioning structures forming arc-shaped curved surfaces. The forging dimensions are designed according to the size requirements of the T-shaped GH4169 rudder shaft forging. The outer contour of the forging is increased by more than 3mm based on the outer contour of the part. At the same time, the diameter D1 of the forging positioning structure and the diameter D2 of the forging rod section satisfy the following conditions: ; 2. Select bar stock; Select bar stock according to the designed forging dimensions, and the diameter of the bar stock should be equal to the diameter D1 of the forging positioning structure; 3. Design molds; design molds based on the designed forgings. The molds include female molds with extrusion nozzles and male molds with punches, and forging is carried out by extrusion and upsetting in one integrated forming method. 4. Forging Simulation: Based on the design in steps 1-3, forging simulation is performed using Deform numerical simulation software. The simulated forging process is as follows: the forging equipment is a screw press, the heating temperature is 1010~1020℃, and the minimum holding time is t. 短 = (0.8 × D1) minutes, longest heating and holding time t 长 = (0.8×D1+90) minutes, where D1 is the maximum effective cross-sectional thickness of the bar stock in mm. The forging process is a single-fire, single-blow process. The transfer time from the billet exiting the heating furnace to the start of forging is controlled to be no more than 30 seconds. During the simulation, the strain value of each part of the forging is not less than 0.6, and the highest temperature of the part in the forging does not exceed 1130℃. If the strain value and the highest temperature requirements are not met, the allowance added when designing the forging is modified and the pits are set in the flat parts until the simulation results meet the requirements. 5. Forging: Forging is carried out according to the forging simulation process that meets the strain value and maximum temperature requirements to obtain the forging. After forging, wait 15 to 20 seconds before demolding and taking out the forging. 6. Heat treatment: Forgings are treated with solution treatment and aging processes; 7. Surface cleaning.
[0006] Its further features are: In step 1, when the widths on both sides of the large end section of the part are inconsistent, the forging is designed symmetrically along the centerline parallel to the length direction; In step 3, the mold also includes a guide sleeve and an ejector rod located at the lower end of the female mold. The ejector rod extends into the female mold through the guide sleeve to eject the forging. In step 6, during solution treatment, the forging is heated to 1010℃ and held for (0.8×D2+60) min, then air-cooled; during aging, it is heated to 720℃ and held for (0.8×D2+480) min, then furnace-cooled to 620℃ and held for (0.8×D2+480) min, then air-cooled. Here, D2 is the maximum effective thickness of the forging in mm. In step 7, the forging is subjected to sandblasting.
[0007] Beneficial effects: The "T"-shaped GH4169 rudder shaft forgings obtained by the above method can effectively ensure uniform grain size of the forgings, while improving material utilization and the efficiency of subsequent product processing. The average grain size of the forgings can reach level 5. In addition, the mold design can achieve demolding through ejector pins, which can solve the problem of difficult demolding of shaft forgings and deformation caused by ejection. The post-forging heat treatment method can significantly improve room temperature impact performance without significant decrease in strength level, enabling the industrial production of forgings with high impact performance requirements. Attached Figure Description
[0008] Figure 1 A schematic diagram of the "T"-shaped GH4169 rudder shaft forging structure; Figure 2 for Figure 1 A bottom view; Figure 3 A schematic diagram of the mold structure designed for step 3; Figure 4 Metallographic diagram of the large section; Figure 5 Metallographic diagram of the connection between the large end section and the rod section; Figure 6 Metallographic diagram of the rod segment; Figure 7 This is a table showing the impact performance. Detailed Implementation
[0009] A method for machining a T-shaped GH4169 high-temperature alloy rudder shaft forging includes the following steps: 1. Designing the forging; such as... Figure 1 , Figure 2 As shown, the "T"-shaped GH4169 rudder shaft forging includes a large end section 100 at the upper end and a columnar rod section 200 at the lower end. The top surface of the large end section 100 is flat, and the cross-section of the large end section 100 is a quadrilateral with rounded corners. Simultaneously, its opposite sides along its length have outwardly protruding positioning structures 300 forming arc-shaped curved surfaces. The diameter D1 of the forging positioning structure 300 is greater than the width L of the large end section. The forging dimensions are designed according to the size requirements of the "T"-shaped GH4169 rudder shaft forging. The outer contour of the forging is increased by more than 3mm based on the outer contour of the part. When the widths on both sides of the large end section are inconsistent ( Figure 1 , 2 The dashed line represents the outline of the part, i.e. Figure 2 When the intermediate dimensions L1 and L2 are inconsistent, the forging is designed symmetrically along the centerline parallel to the length direction to avoid tilting of the final forging due to the asymmetrical structure during the forging process; at the same time, the diameter D1 of the forging positioning structure and the diameter D2 of the forging rod segment satisfy the following conditions: Only under these conditions can the uniform deformation of the forging be guaranteed and forging cracks be prevented.
[0010] 2. Select bar stock; Select bar stock according to the designed forging dimensions. The diameter of the bar stock should be equal to the diameter D1 of the positioning structure of the forging. The raw material bar stock of GH4169 should meet the requirements of technical standard GJB713.
[0011] 3. Mold design; design the mold based on the designed forging, combined with... Figure 3 The mold includes a female mold 2 with an extrusion port device 3, a punch male mold 1, a guide sleeve 4 located at the lower end of the female mold 2, and an ejector rod 5. It is forged by extrusion and upsetting in one piece, which can achieve uniform grain size of the GH4169 "T-type" rudder shaft forging. When demolding, the ejector rod 5 extends from the guide sleeve 4 into the female mold 2 to push out the forging, which facilitates the demolding of the blank after forging.
[0012] 4. Forging Simulation: Based on the design in steps 1-3, forging simulation is performed using Deform numerical simulation software. The simulated forging process is as follows: the forging equipment is a screw press, the heating temperature is 1010~1020℃, and the minimum holding time is t. 短 = (0.8 × D1) minutes, longest heating and holding time t 长 = (0.8 × D1 + 90) minutes, where D1 is the maximum effective cross-sectional thickness of the bar stock in mm. The heating furnace equipment must meet the requirements of Class III electric furnace in HB5425. The forging process is a single-fire, single-blow process. The transfer time of the billet from the heating furnace to the start of forging should not exceed 30 seconds. During the simulation, the strain value of each part of the forging should not be less than 0.6, and the highest temperature of the part in the forging should not exceed 1130℃. Meeting this requirement is the key to obtaining uniform grains. If the strain value and maximum temperature requirements are not met, the allowance added when designing the forging should be modified and a downwardly recessed arc-shaped pit should be set in the flat part until the simulation results meet the requirements.
[0013] 5. Forging: Forging is carried out according to the forging simulation process that meets the strain value and maximum temperature requirements to obtain the forging. After forging, wait 15 to 20 seconds before demolding and taking out the forging.
[0014] 6. Heat Treatment: The forgings are treated with solution treatment and aging processes. During solution treatment, the forgings are heated to 1010℃ and held for (0.8×D2+60) min, then air-cooled. During aging, the forgings are heated to 720℃ and held for (0.8×D2+480) min, then furnace-cooled to 620℃ and held for (0.8×D2+480) min, then air-cooled. D2 is the maximum effective thickness of the forging, in mm. The heating furnace must meet the requirements of Class III electric furnaces in HB5425. The solution temperature selected in this heat treatment process design differs from the solution temperatures specified in common standards (e.g., GJB713, GJB5280, etc.), and is a key parameter for obtaining high impact values in this invention.
[0015] 7. Surface cleaning. After heat treatment, the forgings need to be sandblasted and then transferred for machining.
[0016] The forgings obtained using the above method were sampled and the grain structure was observed. The metallographic image of the large end section is shown below. Figure 4 As shown, the metallographic diagram of the connection between the large end section and the rod section is as follows: Figure 5 As shown, the metallographic diagram of the rod segment is as follows: Figure 6 As shown, the grains are uniform throughout, and the average grain size can reach level 5.
[0017] like Figure 7 As shown, according to traditional processes, rudder shaft forgings are typically produced by first forging into square billets or round bars using multiple heat treatments at temperatures of 995-1060℃, followed by solution treatment at 950-980℃. Two groups of forgings were selected for room temperature tensile and impact tests. Simultaneously, two groups of forgings treated using the method provided in this invention were also selected for room temperature tensile and impact tests. It can be seen that this method significantly improves impact performance while meeting the strength standards and without significant decrease.
[0018] The above are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A method for machining a T-shaped GH4169 high-temperature alloy rudder shaft forging, characterized in that, It includes the following steps:
1. Design the forging; The "T"-shaped GH4169 rudder shaft forging includes a large end section at the top and a columnar rod section at the bottom. The top surface of the large end section is flat, and its cross-section is a quadrilateral with rounded corners. Simultaneously, its opposite sides along its length have outwardly protruding positioning structures forming arc-shaped curved surfaces. Design the forging dimensions according to the dimensional requirements of the "T"-shaped GH4169 rudder shaft forging. The outer contour of the forging should have an allowance of at least 3mm over the outer contour of the part. Furthermore, the diameter D1 of the positioning structure and the diameter D2 of the rod section must satisfy the following conditions: 60%≥(D1 2 -D2 2 ) / D1 2 ≥30%; 2. Select bar stock; Select bar stock according to the designed forging dimensions, and the diameter of the bar stock should be equal to the diameter D1 of the forging positioning structure; 3. Design molds; design molds based on the designed forgings. The molds include female molds with extrusion nozzles and male molds with punches, and forging is carried out by extrusion and upsetting in one integrated forming method.
4. Forging Simulation: Based on the design in steps 1-3, forging simulation is performed using Deform numerical simulation software. The simulated forging process is as follows: the forging equipment is a screw press, the heating temperature is 1010~1020℃, and the minimum holding time is t. 短 = (0.8 × D1') minutes, longest heating and holding time t 长 = (0.8 × D1' + 90) minutes, where D1' is the maximum effective cross-sectional thickness of the bar stock in mm. The forging process is a single-fire, single-blow process. The transfer time from the billet exiting the heating furnace to the start of forging is controlled to be no more than 30 seconds. During the simulation, the strain value of each part of the forging is not less than 0.6, and the highest temperature of the part in the forging does not exceed 1130℃. If the strain value and the highest temperature requirements are not met, the allowance added when designing the forging is modified and the pits are set in the flat parts until the simulation results meet the requirements.
5. Forging: Forging is carried out according to the forging simulation process that meets the strain value and maximum temperature requirements to obtain the forging. After forging, wait 15 to 20 seconds before demolding and taking out the forging.
6. Heat treatment: Forgings are treated with solution treatment and aging processes; In step 6, during solution treatment, the forging is heated to 1010℃ and held for (0.8×D2'+60) min, then air-cooled; during aging, it is heated to 720℃ and held for (0.8×D2'+480) min, then furnace-cooled to 620℃ and held for (0.8×D2'+480) min, then air-cooled, where D2' is the maximum effective thickness of the forging in mm; 7. Surface cleaning; In step 7, the forging is sandblasted.
2. The method for machining a T-shaped GH4169 high-temperature alloy rudder shaft forging according to claim 1, characterized in that: In step 1, when the widths on both sides of the large end section of the part are inconsistent, the forging is designed symmetrically along the centerline parallel to the length direction.
3. The method for machining a T-shaped GH4169 high-temperature alloy rudder shaft forging according to claim 1, characterized in that: In step 3, the mold also includes a guide sleeve and an ejector rod located at the lower end of the female mold. The ejector rod extends from the guide sleeve into the female mold to eject the forging.
Citation Information
Patent Citations
T iron forging and pressing die
CN103611867A
Manufacturing method and manufacturing tooling for T-type forgings
CN106345952A