A corrosion-resistant high-hardness welding wire for CMT surfacing of hydraulic support oil cylinder and a preparation method thereof

By using CMT (Cold Metal Transfer) technology and a high-hardness, corrosion-resistant welding wire composed of powder for CMT welding of hydraulic support cylinder surfaces, the shortcomings of existing technologies such as copper plating and laser cladding are overcome, and a weld overlay layer with excellent corrosion resistance and hardness is prepared, which is suitable for the harsh environment of hydraulic support cylinders.

CN118268756BActive Publication Date: 2026-11-24YULIN UNIVERSITY +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410399679.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-03
Publication Date
2026-11-24
Estimated Expiration
2044-04-03

AI Technical Summary

Technical Problem

In existing technologies, copper plating technology causes environmental pollution, laser cladding technology is costly, and traditional carbon steel and stainless steel overlay welding has a high dilution rate and poor corrosion resistance of the weld layer, which cannot meet the performance requirements of hydraulic support cylinders in harsh service environments.

Method used

The CMT cold metal transfer technology is adopted, using corrosion-resistant high-hardness welding wire for CMT welding of hydraulic support cylinder surface with powder composition including Cr powder, Nb powder, Mo powder, CeO₂+Y₂O₃ powder and Ni powder. The flux-cored welding wire is prepared by vacuum heating, mixing, wrapping and drawing to form a welding layer with low dilution rate.

Benefits of technology

The prepared weld overlay has excellent corrosion resistance and high hardness, making it suitable for the harsh service conditions of hydraulic support cylinders. It is also easy to perform conventional MIG/TIG welding and has strong practical application in engineering.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118268756B_ABST
    Figure CN118268756B_ABST
Patent Text Reader

Abstract

This invention discloses a corrosion-resistant high-hardness welding wire for CMT surfacing of hydraulic support cylinders and its preparation method, comprising flux powder and a welding layer. The flux powder is composed of the following components by mass percentage: Cr powder 60-70%, Nb powder 5-10%, Mo powder 5-10%, CeO2+Y2O3 powder 0.5-1%, and the remainder being Ni powder, with the sum of the mass percentages of the above components being 100%. The flux-cored welding wire of this invention is used for welding with a CMT welding power source, resulting in a weld overlay with high hardness and excellent corrosion resistance, thereby meeting the increasingly harsh service conditions required for hydraulic support cylinders.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metal welding technology, specifically relating to a corrosion-resistant high-hardness welding wire for CMT overlay welding of hydraulic support cylinders and its preparation method. Background Technology

[0002] As a key supporting component in hydraulic supports, the hydraulic cylinder, working in conjunction with the column in an emulsion to complete hydraulic extension and contraction, is prone to failure due to corrosion and wear on its inner wall under repeated pressure and emulsion erosion. Therefore, employing advanced surface treatment processes to enhance the corrosion and wear resistance of the cylinder's inner wall surface is a crucial step in improving the overall performance of hydraulic supports. In recent years, common surface treatment techniques and methods for strengthening the cylinder's inner wall include copper plating, copper fusion, welding of carbon steel and stainless steel, and laser cladding, which can improve the wear and corrosion resistance of the cylinder's inner wall surface to a certain extent.

[0003] With the widespread application of these technologies, various processing methods have revealed certain technical drawbacks. Copper plating technology suffers from environmental pollution, laser cladding technology is costly, and traditional cladding of carbon steel and stainless steel results in poor corrosion resistance due to high dilution rates. The CMT (Cold Metal Transfer) technology, developed in recent years, utilizes a unique wire drawing method to achieve droplet short-circuit transfer under low current, enabling the preparation of cladding layers with low dilution rates, making it an ideal choice for cylinder surface modification. However, due to increasingly harsh downhole operating environments, the performance requirements for cylinder surface layers are also becoming increasingly stringent. Summary of the Invention

[0004] The purpose of this invention is to provide a corrosion-resistant high-hardness welding wire for CMT cladding of hydraulic support cylinders and its preparation method, so as to solve the problems of environmental pollution caused by existing copper plating technology, high cost of laser cladding technology, and poor corrosion resistance of traditional carbon steel and stainless steel cladding due to high dilution rate.

[0005] The present invention adopts the following technical solution: a corrosion-resistant high-hardness welding wire for CMT overlay welding of hydraulic support cylinder surface, comprising flux powder and welding skin, wherein the flux powder comprises the following components by mass percentage: Cr powder 60-70%, Nb powder 5-10%, Mo powder 5-10%, CeO2+Y2O3 powder 0.5-1%, and the remainder is Ni powder, and the sum of the mass percentages of the above components is 100%.

[0006] Preferably, the purity of Cr powder, Nb powder, Mo powder and Ni powder is ≥99.9%.

[0007] Preferably, the particle size of the powder is 100-200 mesh.

[0008] Preferably, the welding skin is made of 304 steel strip with a thickness of 0.3 mm and a width of 7 mm.

[0009] Preferably, the filling amount of the flux-cored welding wire is controlled at 17-19 wt%.

[0010] Another objective of this invention is to provide a method for preparing corrosion-resistant high-hardness welding wire for CMT overlay welding on the surface of a hydraulic support cylinder, the specific steps of which are as follows:

[0011] Step 1: Weigh out Cr, Nb powder, Mo powder, CeO2+Y2O3 powder, and Ni powder according to their respective mass percentages. The sum of the mass percentages of the above components is 100%.

[0012] Step 2: Place the powder weighed in Step 1 into a vacuum heating furnace and heat it at a temperature of 250-280℃ for 1-2 hours to remove the water of crystallization from the powder. After drying, place the powder into a powder mixer for thorough mixing for 1-2 hours.

[0013] Step 3: Use alcohol to remove the grease from the surface of the welding skin, and use a flux-cored wire drawing device to wrap the flux powder prepared in step 2 inside the welding belt to form a coarse welding wire.

[0014] Step 4: The coarse welding wire prepared in Step 3 is drawn repeatedly until it reaches the preset diameter range.

[0015] Step 5: After the flux-cored welding wire is drawn, it is wound onto the welding wire spool by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for later use.

[0016] Preferably, in step 4, the diameter of the first drawing die is 2.6 mm. After the first drawing process is completed, the diameters of the second to Nth dies are reduced sequentially, N≥2, and finally a flux-cored wire with a diameter of 1.2 mm is obtained.

[0017] The beneficial effects of the present invention are as follows: The present invention provides a corrosion-resistant high-hardness welding wire for surfacing hydraulic support cylinders, which uses CMT technology to prepare the surfacing layer on the cylinder surface. The prepared surfacing layer has both excellent corrosion resistance and high hardness, and is used to solve the increasingly harsh service conditions required for hydraulic support cylinders.

[0018] (1) The flux-cored welding wire of the present invention has a relatively small diameter, fewer alloying elements, is simple to prepare, and is convenient for conventional MIG / TIG welding, making it highly applicable to engineering practice.

[0019] (2) The welding wire of the present invention is mainly composed of Cr and Ni elements, which can ensure that the obtained weld overlay has excellent corrosion resistance; Nb, Mo and other strengthening elements are added to the welding wire, and through solid solution strengthening, the high hardness of the cladding layer is achieved.

[0020] (3) The welding wire of this invention contains CeO2+Y2O3 powder. The addition of rare earth elements purifies the grain boundaries of the cladding metal and improves the grain boundary bonding strength. This invention adds rare earth elements in a composite manner, which can ensure the complementary properties of the rare earth elements and makes the effect of refining grains more significant. Attached Figure Description

[0021] Figure 1 The flux-cored wire prepared in Example 2 was used to form a CMT overlay on the surface of a hydraulic support cylinder. The macroscopic morphology of the resulting overlay is shown.

[0022] Figure 2 The flux-cored welding wire prepared in Example 2 was used to build a weld layer on the surface of a hydraulic support cylinder. The metallographic structure of the weld layer interface is shown below.

[0023] Figure 3 The flux-cored welding wire prepared in Example 2 was used to build up a welding layer on the surface of a hydraulic support cylinder. The resulting welding layer has a metallographic structure inside. Detailed Implementation

[0024] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0025] This invention discloses a corrosion-resistant high-hardness welding wire for CMT overlay welding of hydraulic support cylinder surface, comprising flux powder and welding skin, wherein the flux powder comprises the following components by mass percentage: Cr powder 60-70%, Nb powder 5-10%, Mo powder 5-10%, CeO2+Y2O3 powder 0.5-1%, and the remainder is Ni powder, the sum of the mass percentages of the above components being 100%.

[0026] Among them, the purity of Cr powder, Nb powder, Mo powder, and Ni powder is ≥99.9%, and the particle size of Cr powder, Nb powder, Mo powder, CeO2+Y2O3 powder, and Ni powder is 100-200 mesh.

[0027] The welding skin is made of 304 steel strip, with a thickness of 0.3mm and a width of 7mm.

[0028] The filler content of the flux-cored welding wire is controlled at 17-19 wt%.

[0029] The roles and functions of each component in this flux-cored welding wire are as follows:

[0030] (1) As the main alloying element in flux-cored welding wire, Cr is fundamental to determining the corrosion resistance of the cladding metal. Cr can effectively prevent external corrosive media from corroding the substrate by forming a dense Cr2O3 with O. In addition, Cr dissolves in the iron matrix and improves the strength of the iron-based cladding layer through solid solution strengthening.

[0031] (2) As the main alloying element in flux-cored welding wire, the addition of Ni can further improve the corrosion resistance of the cladding metal. Ni can improve the strength and toughness of the iron matrix by solid dissolving in it.

[0032] (3) Nitrogen (Nb) is the main alloying element in welding wire flux. Since Nb has a smaller atomic radius than Fe, its solid solution in the iron matrix can effectively improve the strength of the cladding metal. In addition, Nb is also a strong carbide-forming element, which further improves the strength and hardness of the cladding metal by forming NbC.

[0033] (4) Mo is another major element in welding wire flux. Mo has a more significant solid solution strengthening effect than Nb. In addition, the addition of Mo can further improve the corrosion resistance of the cladding metal.

[0034] (5) The addition of CeO2+Y2O3 oxides can purify the grain boundaries of the weld and improve the grain boundary bonding force, thereby improving the plasticity and toughness of iron-based cladding metal.

[0035] The specific steps of the above-mentioned method for preparing corrosion-resistant high-hardness welding wire for CMT overlay welding on the surface of hydraulic support cylinder are as follows:

[0036] Step 1: Weigh out 60-70% Cr powder, 5-10% Nb powder, 5-10% Mo powder, 0.5-1% CeO2+Y2O3 powder, and the remainder Ni powder by mass percentage. The sum of the mass percentages of the above components is 100%.

[0037] Step 2: Place the powder weighed in Step 1 into a vacuum heating furnace and heat it at a temperature of 250-280℃ for 1-2 hours to remove the water of crystallization from the powder. After drying, place the powder into a powder mixer for thorough mixing for 1-2 hours.

[0038] Step 3: Use alcohol to remove the grease from the surface of the 304 steel strip, and use a flux-cored wire drawing device to wrap the flux powder prepared in step 2 inside the 304 steel strip. The diameter of the first drawing die is 2.6mm.

[0039] Step 4: After the first drawing process is completed, the die hole diameter is changed to 2.5mm, 2.3mm, 2.1mm, 1.9mm, 1.7mm, 1.6mm, 1.5mm, 1.4mm, 1.3mm and 1.2mm respectively for drawing. The final diameter of the flux-cored wire is 1.2mm.

[0040] Step 5: After the flux-cored welding wire is drawn, it is wound onto the welding wire spool by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for later use.

[0041] In step 1, the purity of Cr powder, Nb powder, Mo powder, and Ni powder is ≥99.9%, and the particle size of Cr powder, Nb powder, Mo powder, CeO2+Y2O3 powder, and Ni powder is 100-200 mesh.

[0042] In step 3, the welding skin is made of 304 steel strip with a thickness of 0.3mm and a width of 7mm.

[0043] In step 3, the filling amount of flux-cored welding wire is controlled at 17-19 wt%.

[0044] Example 1

[0045] Step 1: Weigh out 60% Cr powder, 5% Nb powder, 5% Mo powder, 0.5% CeO2+Y2O3 powder, and the remainder Ni powder by mass percentage. The sum of the mass percentages of the above components is 100%.

[0046] Step 2: Place the powder weighed in Step 1 into a vacuum heating furnace and heat it at 250℃ for 1 hour to remove the water of crystallization from the powder. After drying, place the powder into a powder mixer for thorough mixing for 1 hour.

[0047] Step 3: Use alcohol to remove the grease from the surface of the 304 steel strip, and use a flux-cored wire drawing device to wrap the flux powder prepared in step 2 inside the 304 steel strip. The diameter of the first drawing die is 2.6mm.

[0048] Step 4: After the first drawing process is completed, the die hole diameter is changed to 2.5mm, 2.3mm, 2.1mm, 1.9mm, 1.7mm, 1.6mm, 1.5mm, 1.4mm, 1.3mm and 1.2mm respectively for drawing. The final diameter of the flux-cored wire is 1.2mm.

[0049] Step 5: After the flux-cored welding wire is drawn, it is wound onto the welding wire spool by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for later use.

[0050] The corrosion-resistant high-hardness welding wire for CMT surfacing of the hydraulic support cylinder prepared in Example 1 was used for MIG welding with a CMT welding power source. No preheating was required before welding. The welding current was 180-210 A, the shielding gas was 98% Ar + 2% O2, and the gas flow rate was 15-18 L / min. The experimental results are as follows:

[0051] (1) The weld overlay is aesthetically pleasing and no cracks or defects were found in the penetrant test;

[0052] (2) The weld overlay is well bonded to the hydraulic support cylinder base. The weld overlay structure is mainly martensitic with fine lath bundles. No defects were found inside the weld overlay.

[0053] (3) The average micro Vickers hardness of the weld overlay is 540 HV0.2;

[0054] (4) The weld overlay does not rust after 440 hours in a neutral salt spray environment.

[0055] Example 2

[0056] Step 1: Weigh out 70% Cr powder, 10% Nb powder, 10% Mo powder, 1% CeO2+Y2O3 powder, and the remainder Ni powder by mass percentage. The sum of the mass percentages of the above components is 100%.

[0057] Step 2: Place the powder weighed in Step 1 into a vacuum heating furnace and heat it at 280℃ for 2 hours to remove the water of crystallization from the powder. After drying, place the powder into a powder mixer for thorough mixing for 2 hours.

[0058] Step 3: Use alcohol to remove the grease from the surface of the 304 steel strip, and use a flux-cored wire drawing device to wrap the flux powder prepared in step 2 inside the 304 steel strip. The diameter of the first drawing die is 2.6mm.

[0059] Step 4: After the first drawing process is completed, the die hole diameter is changed to 2.5mm, 2.3mm, 2.1mm, 1.9mm, 1.7mm, 1.6mm, 1.5mm, 1.4mm, 1.3mm and 1.2mm respectively for drawing. The final diameter of the flux-cored wire is 1.2mm.

[0060] Step 5: After the flux-cored welding wire is drawn, it is wound onto the welding wire spool by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for later use.

[0061] The corrosion-resistant, high-hardness welding wire for CMT surfacing of the hydraulic support cylinder prepared in Example 2 was used for MIG welding with a CMT welding power source. No preheating was required before welding. The welding current was 180-210 A, the shielding gas was 98% Ar + 2% O2, and the gas flow rate was 15-18 L / min. The experimental results are as follows:

[0062] (1) The weld overlay is aesthetically pleasing and no cracks or defects were found in the penetrant test;

[0063] (2) The weld overlay is well bonded to the hydraulic support cylinder base. The weld overlay structure is mainly martensitic with fine lath bundles. No defects were found inside the weld overlay.

[0064] (3) The average micro Vickers hardness of the weld overlay is 570 HV0.2;

[0065] (4) The weld overlay does not rust after 400 hours in a neutral salt spray environment.

[0066] Figure 1 The macroscopic morphology of the weld overlay obtained by welding the flux-cored wire prepared for Case 2 onto the surface of the hydraulic support cylinder is shown in the figure. It can be seen from the figure that the weld overlay is aesthetically pleasing.

[0067] Figure 2 The image shows the low-magnification microstructure at the interface between the weld overlay and the hydraulic support cylinder. As can be seen from the image, there are no defects at the interface, and the weld overlay is mainly composed of columnar dendrites.

[0068] Figure 3 The image shows the metallographic morphology inside the weld overlay layer. As can be seen from the image, the dendrites are relatively fine.

[0069] Example 3

[0070] Step 1: Weigh out 65% Cr powder, 7% Nb powder, 7% Mo powder, 0.8% CeO2+Y2O3 powder, and the remainder Ni powder by mass percentage. The sum of the mass percentages of the above components is 100%.

[0071] Step 2: Place the powder weighed in Step 1 into a vacuum heating furnace and heat it at 270℃ for 1.5 hours to remove the water of crystallization from the powder. After drying, place the powder into a powder mixer and mix it thoroughly for 1.5 hours.

[0072] Step 3: Use alcohol to remove the grease from the surface of the 304 steel strip, and use a flux-cored wire drawing device to wrap the flux powder prepared in step 2 inside the 304 steel strip. The diameter of the first drawing die is 2.6mm.

[0073] Step 4: After the first drawing process is completed, the die hole diameter is changed to 2.5mm, 2.3mm, 2.1mm, 1.9mm, 1.7mm, 1.6mm, 1.5mm, 1.4mm, 1.3mm and 1.2mm respectively for drawing. The final diameter of the flux-cored wire is 1.2mm.

[0074] Step 5: After the flux-cored welding wire is drawn, it is wound onto the welding wire spool by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for later use.

[0075] The corrosion-resistant high-hardness welding wire for CMT surfacing of the hydraulic support cylinder prepared in Example 3 was used for MIG welding with a CMT welding power source. No preheating was required before welding. The welding current was 180-210 A, the shielding gas was 98% Ar + 2% O2, and the gas flow rate was 15-18 L / min. The experimental results are as follows:

[0076] (1) The weld overlay is aesthetically pleasing and no cracks or defects were found in the penetrant test;

[0077] (2) The weld overlay is well bonded to the hydraulic support cylinder base. The weld overlay structure is mainly martensitic with fine lath bundles. No defects were found inside the weld overlay.

[0078] (3) The average micro Vickers hardness of the weld overlay is 582 HV0.2;

[0079] (4) The weld overlay does not rust after 450 hours in a neutral salt spray environment.

[0080] Example 4

[0081] Step 1: Weigh out 67% Cr powder, 8% Nb powder, 8% Mo powder, 0.6% CeO2+Y2O3 powder, and the remainder is Ni powder according to the following mass percentages. The sum of the mass percentages of the above components is 100%.

[0082] Step 2: Place the powder weighed in Step 1 into a vacuum heating furnace and heat it at 260℃ for 1.2 hours to remove the water of crystallization from the powder. After drying, place the powder into a powder mixer for thorough mixing for 1.2 hours.

[0083] Step 3: Use alcohol to remove the grease from the surface of the 304 steel strip, and use a flux-cored wire drawing device to wrap the flux powder prepared in step 2 inside the 304 steel strip. The diameter of the first drawing die is 2.6mm.

[0084] Step 4: After the first drawing process is completed, the die hole diameter is changed to 2.5mm, 2.3mm, 2.1mm, 1.9mm, 1.7mm, 1.6mm, 1.5mm, 1.4mm, 1.3mm and 1.2mm respectively for drawing. The final diameter of the flux-cored wire is 1.2mm.

[0085] Step 5: After the flux-cored welding wire is drawn, it is wound onto the welding wire spool by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for later use.

[0086] The corrosion-resistant, high-hardness welding wire for CMT surfacing of the hydraulic support cylinder prepared in Example 4 was used for MIG welding with a CMT welding power source. No preheating was required before welding. The welding current was 180-210 A, the shielding gas was 98% Ar + 2% O2, and the gas flow rate was 15-18 L / min. The experimental results are as follows:

[0087] (1) The weld overlay is aesthetically pleasing and no cracks or defects were found in the penetrant test;

[0088] (2) The weld overlay is well bonded to the hydraulic support cylinder base. The weld overlay structure is mainly martensitic with fine lath bundles. No defects were found inside the weld overlay.

[0089] (3) The average micro Vickers hardness of the weld overlay is 555 HV0.2;

[0090] (4) The weld overlay does not rust in a neutral salt spray environment for 410 hours.

[0091] Example 5

[0092] Step 1: Weigh out 61% Cr powder, 9% Nb powder, 9% Mo powder, 0.9% CeO2+Y2O3 powder, and the remainder is Ni powder according to the following mass percentages. The sum of the mass percentages of the above components is 100%.

[0093] Step 2: Place the powder weighed in Step 1 into a vacuum heating furnace and heat it at 255℃ for 1.7 hours to remove the water of crystallization from the powder. After drying, place the powder into a powder mixer for thorough mixing for 1.3 hours.

[0094] Step 3: Use alcohol to remove the grease from the surface of the 304 steel strip, and use a flux-cored wire drawing device to wrap the flux powder prepared in step 2 inside the 304 steel strip. The diameter of the first drawing die is 2.6mm.

[0095] Step 4: After the first drawing process is completed, the die hole diameter is changed to 2.5mm, 2.3mm, 2.1mm, 1.9mm, 1.7mm, 1.6mm, 1.5mm, 1.4mm, 1.3mm and 1.2mm respectively for drawing. The final diameter of the flux-cored wire is 1.2mm.

[0096] Step 5: After the flux-cored welding wire is drawn, it is wound onto the welding wire spool by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for later use.

[0097] The corrosion-resistant, high-hardness welding wire for CMT surfacing of the hydraulic support cylinder prepared in Example 5 was used for MIG welding with a CMT welding power source. No preheating was required before welding. The welding current was 180-210 A, the shielding gas was 98% Ar + 2% O2, and the gas flow rate was 15-18 L / min. The experimental results are as follows:

[0098] (1) The weld overlay is aesthetically pleasing and no cracks or defects were found in the penetrant test;

[0099] (2) The weld overlay is well bonded to the hydraulic support cylinder base. The weld overlay structure is mainly martensitic with fine lath bundles. No defects were found inside the weld overlay.

[0100] (3) The average micro Vickers hardness of the weld overlay is 594 HV0.2;

[0101] (4) The weld overlay does not rust in a neutral salt spray environment for 460 hours.

[0102] The existing weld overlay corrodes within 24 hours in a neutral salt spray environment.

[0103] Although the present invention has been described in detail through the preferred embodiments above, it should be understood that the above description should not be considered as a limitation of the present invention. Various modifications and substitutions to the present invention will be apparent to those skilled in the art after reading the above description. Therefore, the scope of protection of the present invention should be defined by the appended claims.

Claims

1. A corrosion-resistant high-hardness welding wire for CMT overlay welding on the surface of a hydraulic support cylinder, comprising flux powder and welding scale, characterized in that: The powder comprises the following components by mass percentage: Cr powder 60-70%, Nb powder 5-10%, Mo powder 5-10%, CeO2+Y2O3 powder 0.5-1%, and the remainder is Ni powder. The sum of the mass percentages of the above components is 100%, and the filling amount of the welding wire is controlled at 17-19 wt%.

2. The corrosion-resistant high-hardness welding wire for CMT overlay welding of hydraulic support cylinder surface as described in claim 1, characterized in that, The purity of the Cr powder, Nb powder, Mo powder and Ni powder is ≥99.9%.

3. The corrosion-resistant high-hardness welding wire for CMT overlay welding of hydraulic support cylinder surface as described in claim 1, characterized in that, The particle size of the powder is 100-200 mesh.

4. The corrosion-resistant high-hardness welding wire for CMT overlay welding of hydraulic support cylinder surface as described in claim 1, characterized in that, The welding skin is made of 304 steel strip, with a thickness of 0.3mm and a width of 7mm.

5. A method for preparing corrosion-resistant high-hardness welding wire for CMT overlay welding on the surface of a hydraulic support cylinder as described in any one of claims 1-4, characterized in that, The specific steps are as follows: Step 1: Weigh out Cr, Nb powder, Mo powder, CeO2+Y2O3 powder, and Ni powder according to the mass percentages specified in claim 1, with the sum of the mass percentages of the above components being 100%. Step 2: Place the powder weighed in Step 1 into a vacuum heating furnace and heat it at a temperature of 250~280℃ for 1~2 hours to remove the water of crystallization from the powder; place the dried powder into a powder mixer for thorough mixing for 1~2 hours. Step 3: Use alcohol to remove the grease from the surface of the weld bead, and use a flux-cored wire drawing device to wrap the flux powder prepared in step 2 inside the welding belt to form a coarse welding wire; Step 4: The coarse welding wire prepared in Step 3 is drawn multiple times until it reaches a preset diameter range; Step 5: After the flux-cored welding wire is drawn, it is wound onto the welding wire spool by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for later use.

6. The method for preparing corrosion-resistant high-hardness welding wire for CMT overlay welding on the surface of hydraulic support cylinder as described in claim 5, characterized in that, In step 4, the diameter of the first drawing die is 2.6 mm. After the first drawing process is completed, the diameters of the second to Nth dies are reduced sequentially, with N≥2, to finally obtain a flux-cored wire with a diameter of 1.2 mm.

Citation Information

Patent Citations

  • Nickel-steel composite material electric arc 3D printing welding wire and preparation and additive manufacturing method

    CN114535859A