High-performance recycled sbs modified asphalt and preparation method thereof

By adding aromatic oils, polycyclic aromatic compounds, and dioxazoline compounds to aged SBS modified asphalt, the cross-linked network structure of SBS polymer is reconstructed, solving the problem of poor performance recovery during the recycling process of SBS modified asphalt, meeting the requirements for use in high-grade highways, and reducing environmental and health risks.

CN118271863BActive Publication Date: 2026-11-20HARBIN INST OF TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410506967.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-25
Publication Date
2026-11-20
Estimated Expiration
2044-04-25

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively restore the performance of SBS modified asphalt, especially the cross-linked network structure of SBS polymers, which results in poor performance recovery of waste SBS modified asphalt during the recycling process, failing to meet the requirements for use on high-grade highways.

Method used

Aromatic oils are used as component regulators, polycyclic aromatic compounds or dioxazoline compounds as SBS structure regenerators, acid anhydrides as compatibilizers, and sulfur as stabilizers. The cross-linked network structure of SBS polymers is reconstructed by heating and stirring, and the reaction is carried out at high temperature to restore the properties of asphalt.

Benefits of technology

This approach fully restores the high and low temperature road performance of SBS modified asphalt, improves the utilization level of waste SBS modified asphalt, reduces environmental pollution, increases material utilization, and reduces health risks to construction workers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004810601570000091
    Figure BDA0004810601570000091
Patent Text Reader

Abstract

The application discloses a kind of high-performance regenerated SBS modified asphalt and preparation method thereof, the regenerated SBS modified asphalt is prepared by aging SBS modified asphalt, component regulator, SBS structure regenerant, compatibilizer, stabilizer, and wherein: component regulator is aromatic oil, SBS structure regenerant is at least one of polycyclic epoxy group compound or dioxazoline compound, compatibilizer is acid anhydride compound, and stabilizer is sulfur.The application makes that the component of regenerated asphalt is not only adjusted, wherein the crosslinked structure of SBS polymer is also reconstructed, and the performance of aged SBS modified asphalt can be restored to high level.The high-performance SBS modified asphalt of the application is comprehensively recovered in high and low temperature road performance, and is superior to original SBS modified asphalt, and can effectively improve the utilization level of waste SBS modified asphalt material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of road engineering material recycling, and relates to a modified asphalt and its preparation method, particularly a high-performance recycled SBS modified asphalt and its preparation method. Background Technology

[0002] In 2021, the Ministry of Transport proposed a target of over 90% recycling rate for old road surface materials in reconstruction, expansion, repair, and maintenance projects nationwide. Currently, SBS modified asphalt is widely used in the pavement of high-grade highways in my country. With early highways entering major repair and reconstruction phases, a large amount of waste SBS modified asphalt mixtures are generated, and the reuse of these waste materials has become a priority. During the aging process of SBS modified asphalt, not only does the base asphalt undergo oxidation, but SBS also degrades, and the cross-linked network structure of the SBS polymer disappears. Therefore, when regenerating SBS modified asphalt, to restore the asphalt performance to a high level as much as possible, it is necessary not only to restore the performance of the base asphalt but also to reconstruct the structure of the SBS modifier.

[0003] Currently, research on the recycling of ordinary asphalt pavements is relatively mature and systematic, with the "Technical Specification for Recycling of Highway Asphalt Pavements" available for reference. However, research on the recycling of SBS modified asphalt pavements is still in the exploratory stage. Conventional asphalt recycling methods aim to restore the performance of the base asphalt by adding low-viscosity oils (such as vegetable oil, catalytic cracking slurry, and waste engine oil) to aged asphalt to adjust the composition of the base asphalt. However, these methods cannot repair or rebuild the degradation products of SBS copolymers. This means that waste SBS modified asphalt can only be recycled as ordinary asphalt, obscuring the value of SBS itself and severely affecting the recovery effect of SBS modified asphalt performance.

[0004] In recent years, some studies have focused on restoring the performance of SBS-modified asphalt by reconstructing the molecular structure of SBS in aged asphalt. This has been achieved through the use of diepoxy glycidyl ether compounds (such as 1,4-butanediol diglycidyl ether and 1,6-hexanediol diglycidyl ether) or diisocyanate compounds (such as 4,4'-diphenyldimethyl diisocyanate, hexamethylene diisocyanate, and toluene diisocyanate) for SBS structural regeneration. However, diepoxy glycidyl ether compounds have low reactivity, and even with the addition of catalysts, it is difficult to reconstruct the cross-linked network structure of the SBS polymer, resulting in the inability to restore the performance of SBS-modified asphalt to its original high level. Furthermore, diisocyanate compounds are highly toxic, and their vapors in the air can cause significant irritation to the respiratory tract and eyes. The high temperatures often encountered during asphalt processing further promote the volatilization of diisocyanate compounds. Therefore, diisocyanate compounds are not suitable for the actual production of SBS-modified asphalt regeneration. To improve the utilization level of waste SBS modified asphalt and enable the recycled asphalt to still be used in high-grade highways, it is necessary to further explore recycling methods for aged SBS modified asphalt. Summary of the Invention

[0005] To address the aforementioned shortcomings of existing technologies, this invention provides a high-performance recycled SBS-modified asphalt and its preparation method. This method not only adjusts the composition of the recycled asphalt but also reconstructs the cross-linked network structure of the SBS polymer, allowing the performance of aged SBS-modified asphalt to be restored to a high level. The high-performance SBS-modified asphalt of this invention fully restores its high and low temperature road performance, surpassing that of undiluted SBS-modified asphalt, effectively improving the utilization level of waste SBS-modified asphalt materials.

[0006] The objective of this invention is achieved through the following technical solution:

[0007] A high-performance recycled SBS modified asphalt is prepared from 100 parts by weight of aged SBS modified asphalt, 6-10 parts by weight of component modifier, 0.2-0.7 parts by weight of SBS structural regenerator, 0.1-0.3 parts by weight of compatibilizer, and 0.15-0.25 parts by weight of stabilizer, wherein:

[0008] The component modifier is an aromatic oil, and the kinematic viscosity of the aromatic oil at 100°C is 36.13 mm. 2 / s, moisture content 0.06%, density 0.9511g / cm³ 3 ;

[0009] The SBS structure regenerator is at least one of a polyepoxy group compound or a dioxazoline compound;

[0010] The polyepoxy group compound is at least one of glycerol triglycidyl ether and N,N,N,N,N-tetragoxypropyl-4,4-diaminodiphenylmethane;

[0011] The dioxazoline compound is 2,2'-(1,3-phenylene)-dioxazoline;

[0012] The compatibilizer is an acid anhydride compound;

[0013] The acid anhydride compound is maleic anhydride or phthalic anhydride;

[0014] The stabilizer is sulfur.

[0015] A method for preparing the above-mentioned high-performance recycled SBS modified bitumen includes the following steps:

[0016] Step (1) Heat the aged SBS modified asphalt to 130-160℃, and add component regulator and compatibilizer at a stirring speed of 1000-1200r / min, and continue stirring for 3-5min.

[0017] Step (2) Add SBS structure regenerator at the same temperature and speed, and continue stirring for 15-20 minutes;

[0018] Step (3) Add stabilizer at the same temperature and speed, and continue stirring for 10-15 minutes;

[0019] Step (4) Place the sample that has been stirred in step (3) in an environment of 120-140℃ for 20-40 minutes to develop. After development, cool to room temperature to obtain high-performance recycled SBS modified asphalt.

[0020] Compared with existing technologies, the present invention has the following advantages:

[0021] (1) During the aging process of SBS modified asphalt, the aromatic components in the asphalt will transform into resins and asphaltenes, and the SBS polymer will be oxidized and degraded into small molecules. By adding component regulators such as aromatic oils, the light components of aged asphalt can be replenished, thereby restoring the colloidal structure of the asphalt and realizing the regeneration of the base asphalt. Meanwhile, SBS structure regenerators composed of polyepoxy groups and bisoxazoline compounds can react with the hydroxyl and carboxyl groups in the oxidized and degraded SBS small molecules, thereby connecting the SBS small molecules and reconstructing the molecular structure of SBS. Moreover, these two types of compounds have high reactivity with carboxyl groups and fast reaction rates, and no catalyst needs to be added during the reaction. By adding component regulators and SBS structure regenerators to aged SBS modified asphalt, the performance of both the base asphalt and the SBS modifier can be restored simultaneously, resulting in high-performance recycled SBS modified asphalt with excellent high and low temperature road performance. This allows the recycled SBS modified asphalt to be applied to high-grade pavements and extend the service life of the pavement, resulting in significant engineering benefits.

[0022] (2) SBS structure regenerators composed of polyepoxy groups and bisoxazoline compounds have low toxicity and will not have a negative impact on the health and safety of construction workers. Moreover, the direct product of the reaction process is water, not carbon dioxide. In contrast, the direct product of the reaction between diisocyanate compounds and aged SBS is carbon dioxide. Therefore, its reaction is more environmentally friendly than that of diisocyanate SBS structure regenerators.

[0023] (3) In the process of preparing recycled SBS modified asphalt, by adding component regulator and SBS structure regenerator at the same time, the component regulator can act as a penetrant, making it easier for the SBS structure regenerator to penetrate into the aged SBS modified asphalt. After the SBS molecular structure is reconstructed, it is also easier to absorb the surrounding light components, causing the SBS polymer to swell and form a cross-linked network structure in the asphalt.

[0024] (4) By adding a compatibilizer, the hydroxyl groups in aged SBS can be converted into carboxyl groups, resulting in a better reaction between the SBS structure regenerator and aged SBS, and further improving the asphalt performance. Adding a stabilizer helps to ensure that the regenerated SBS is more uniformly and stably dispersed in the asphalt, preventing excessively rapid segregation between the regenerated SBS and the asphalt. By developing the asphalt in an oven at 120–140°C for 20–40 minutes, the reacted SBS polymer can fully develop and swell. At the same time, the moderate temperature also avoids the branching reaction between the SBS structure regenerator and other components in the SBS-modified asphalt during the swelling process, preventing the formation of a gel structure.

[0025] (5) The preparation of high-performance recycled SBS modified asphalt can reduce the amount of new asphalt and new SBS used in actual engineering, improve the utilization rate of waste materials, reduce the waste of waste SBS modified asphalt mixture and the occupation of storage sites, and reduce the pollution caused to the environment to a certain extent. It is of great significance to promote the green development of transportation infrastructure. Detailed Implementation

[0026] The present invention will be further described in detail below with reference to embodiments and comparative examples, but it is not limited thereto. Any modifications or equivalent substitutions to the present technical solution, as long as they do not depart from the spirit and scope of the present invention, should be included within the protection scope of the present invention.

[0027] The physical properties of the recycled SBS modified asphalt prepared in all embodiments and comparative examples of this invention were tested according to the standard "Asphalt and Asphalt Mixtures for Highway Engineering" (JTJE20-2011). The test results are listed in Table 1 for easy comparison.

[0028] In the following examples and comparative examples, SBS modified asphalt (penetration of 45.8 dmm at 25℃, softening point of 73.9℃, ductility of 34.9 cm at 5℃, and viscosity of 2072 mPa·s at 135℃) was first subjected to a film heating test (TFOT), i.e., heated in a film oven at 163℃ for 5 hours, and then subjected to a pressure aging vessel accelerated asphalt aging test (PAV), i.e., aged in a pressure aging chamber at 100℃ and 2.1 MPa for 20 hours, to obtain aged SBS modified asphalt. The properties of the aged SBS modified asphalt are as follows: penetration of 24.6 dmm at 25℃, softening point of 81.3℃, ductility of 2 cm at 5℃, and viscosity of 3174 mPa·s.

[0029] Example 1:

[0030] (1) Weigh 200g of aged SBS modified bitumen, 12g of aromatic oil, 0.4g of glycerol triglycidyl ether, 0.2g of maleic anhydride, and 0.4g of sulfur.

[0031] (2) Heat the aged SBS modified asphalt to 130°C using a closed electric furnace, add aromatic oil and maleic anhydride to the asphalt at the same time, stir for 5 minutes at 1000 r / min using an electric mixer, then add glycerol triglycidyl ether and continue stirring for 15 minutes. After completion, add sulfur and stir for 10 minutes.

[0032] (3) Place the fully mixed asphalt in an oven at 120°C for 40 minutes to develop and obtain high-performance recycled SBS modified asphalt.

[0033] Example 2:

[0034] (1) Weigh 200g of aged SBS modified bitumen, 12g of aromatic oil, 1g of glycerol triglycidyl ether, 0.4g of phthalic anhydride, and 0.5g of sulfur.

[0035] (2) Heat the aged SBS modified asphalt to 130°C using a closed electric furnace, add aromatic oil and maleic anhydride to the asphalt at the same time, stir for 5 minutes at 1000 r / min using an electric mixer, then add glycerol triglycidyl ether and continue stirring for 20 minutes. After completion, add sulfur and stir for 15 minutes.

[0036] (3) Place the fully mixed asphalt in an oven at 130°C for 30 minutes to develop and obtain high-performance recycled SBS modified asphalt.

[0037] Example 3:

[0038] (1) Weigh 200g of aged SBS modified bitumen, 12g of aromatic oil, 1g of N,N,N,N-tetracyclooxypropyl-4,4-diaminodiphenylmethane, 0.4g of phthalic anhydride, and 0.5g of sulfur.

[0039] (2) Heat the aged SBS modified asphalt to 140°C using a closed electric furnace, add aromatic oil and phthalic anhydride to the asphalt at the same time, stir with an electric mixer at 1200 r / min for 3 min, then add N,N,N,N-tetracyclooxypropyl-4,4-diaminodiphenylmethane and continue stirring for 20 min. After completion, add sulfur and stir for 15 min.

[0040] (3) Place the fully mixed asphalt in an oven at 130°C for 30 minutes to develop, and obtain high-performance recycled SBS modified asphalt.

[0041] Example 4:

[0042] (1) Weigh 200g of aged SBS modified bitumen, 16g of aromatic oil, 1g of glycerol triglycidyl ether, 0.4g of phthalic anhydride, and 0.3g of sulfur.

[0043] (2) Heat the aged SBS modified asphalt to 150°C using a closed electric furnace, add aromatic oil and phthalic anhydride to the asphalt at the same time, stir for 5 minutes at 1000 r / min using an electric mixer, then add glycerol triglycidyl ether and stir for 15 minutes. After completion, add sulfur and continue stirring for 10 minutes.

[0044] (3) Place the fully mixed asphalt in an oven at 140°C for 20 minutes to develop, and obtain high-performance recycled SBS modified asphalt.

[0045] Example 5:

[0046] (1) Weigh 200g of aged SBS modified asphalt, 16g of aromatic oil, 1.4g of N,N,N,N-tetracyclooxypropyl-4,4-diaminodiphenylmethane, 0.6g of maleic anhydride, and 0.3g of sulfur.

[0047] (2) Heat the aged SBS modified asphalt to 150°C using a closed electric furnace. Add aromatic oil and maleic anhydride to the asphalt at the same time. Stir for 5 minutes at 1000 r / min using an electric mixer. Then, add N,N,N,N-tetracyclooxypropyl-4,4-diaminodiphenylmethane and stir for 15 minutes. After completion, add sulfur and continue stirring for 10 minutes.

[0048] (3) Place the fully mixed asphalt in an oven at 140°C for 20 minutes to develop, and obtain high-performance recycled SBS modified asphalt.

[0049] Example 6:

[0050] (1) Weigh 200g of aged SBS modified asphalt, 16g of aromatic oil, 0.4g of 2,2'-(1,3-phenylene)-dioxazoline, 0.2g of phthalic anhydride, and 0.5g of sulfur;

[0051] (2) Heat the aged SBS modified asphalt to 140°C using a closed electric furnace, add aromatic oil and phthalic acid glycosides to the asphalt at the same time, stir with an electric mixer at 1200 r / min for 5 min, then add 2,2'-(1,3-phenylene)-dioxazoline and stir for 15 min, then add sulfur and continue stirring for 10 min.

[0052] (3) Place the fully mixed asphalt in an oven at 130°C for 20 minutes to develop, and obtain high-performance recycled SBS modified asphalt.

[0053] Example 7:

[0054] (1) Weigh 200g of aged SBS modified asphalt, 20g of aromatic oil, 1.4g of 2,2'-(1,3-phenylene)-dioxazoline, 0.4g of maleic anhydride, and 0.5g of sulfur;

[0055] (2) Heat the aged SBS modified asphalt to 140°C using a closed electric furnace, add aromatic oil and maleic anhydride to the asphalt at the same time, stir with an electric mixer at 1000 r / min for 5 min, then add 2,2'-(1,3-phenylene)-dioxazoline, and after completion, add sulfur and continue stirring for 10 min.

[0056] (3) Place the fully mixed asphalt in an oven at 120°C for 20 minutes to develop, and obtain high-performance recycled SBS modified asphalt.

[0057] Example 8:

[0058] (1) Weigh 200g of aged SBS modified bitumen, 20g of aromatic oil, 1.4g of N,N,N,N-tetracyclooxypropyl-4,4-diaminodiphenylmethane, 0.6g of phthalic anhydride, and 0.5g of sulfur.

[0059] (2) Heat the aged SBS modified asphalt to 140°C using a closed electric furnace. Add aromatic oil and phthalic anhydride to the asphalt at the same time. Stir for 5 minutes at 1000 r / min using an electric mixer. Then, add N,N,N,N,-tetracyclooxypropyl-4,4-diaminodiphenylmethane and stir for 15 minutes. After completion, add sulfur and continue stirring for 10 minutes.

[0060] (3) Place the fully mixed asphalt in an oven at 120°C for 20 minutes to develop, and obtain high-performance recycled SBS modified asphalt.

[0061] Comparative Example 1:

[0062] (1) Weigh 200g of aged SBS modified bitumen, 20g of aromatic oil, and 0.5g of sulfur;

[0063] (2) Heat the aged SBS modified asphalt to 140°C using a closed electric furnace, add aromatic oil to the asphalt, stir for 20 minutes at a speed of 1000 r / min using an electric mixer, add sulfur and continue stirring for 10 minutes.

[0064] (3) Place the fully mixed asphalt in an oven at 140°C for 20 minutes to develop, and obtain recycled SBS modified asphalt.

[0065] Comparative Example 2:

[0066] (1) Weigh 200g of aged SBS modified asphalt, 20g of aromatic oil, 6g of diepoxy glycidyl ether compound 1,6-hexanediol diglycidyl ether, 0.2g of catalyst |N|,|N|-dimethylbenzylamine, and 0.5g of sulfur;

[0067] (2) Heat the aged SBS modified asphalt to 140°C using a closed electric furnace. Add aromatic oil, 1,6-hexanediol diglycidyl ether, and |N|,|N|-dimethylbenzylamine to the asphalt at the same time. Stir with an electric mixer at 1000 r / min for 20 min. After completion, add sulfur and continue stirring for 10 min.

[0068] (3) Place the fully mixed asphalt in an oven at 140°C for 20 minutes to develop, and obtain recycled SBS modified asphalt.

[0069] Table 1. Test results of three major indicators of recycled SBS modified asphalt in each example and comparative example.

[0070]

[0071] As shown in Table 1, when only the component modifier was added to the aged SBS modified asphalt (Comparative Example 1), the penetration and ductility of the recycled SBS modified asphalt increased, while the softening point decreased, indicating a certain degree of recovery in asphalt performance. However, when both the component modifier and the SBS structural regenerator were added simultaneously, the softening point and ductility of Examples 1-8 all increased compared to Comparative Example 1. This is because the addition of the SBS structural regenerator to the aged SBS modified asphalt repaired the cross-linked network structure of the SBS modified asphalt, thus improving the high and low temperature performance of the recycled SBS modified asphalt. Furthermore, the softening point and ductility of the recycled SBS modified asphalt in Examples 1-8 were also higher than those of the original SBS modified asphalt, and all met the requirements of Class ID unaged SBS modified asphalt in the specification: ductility ≥20 and softening point ≥60, indicating that the high-performance recycled SBS modified asphalt has superior road performance. When glycidyl ether compounds of diepoxy were used as SBS structure regenerators (Comparative Example 2), although the properties of the regenerated SBS modified asphalt were restored, its softening point was lower than that of Comparative Example 1 and did not exceed the level of the original SBS modified asphalt. This is because epoxy regenerators have low activity and cannot react completely after being added. Their ability to repair the network structure of SBS modified asphalt is poor, and they cannot improve the performance of SBS modified asphalt to a higher level.

[0072] In summary, by using the component regulator, SBS structure regenerator, and stabilizer disclosed in this invention, the high and low temperature road performance of aged SBS modified asphalt can be restored and improved to a high level, making it suitable for high-quality engineering applications.

Claims

1. A high-performance recycled SBS modified bitumen, characterized in that... The recycled SBS modified asphalt is prepared from 100 parts by weight of aged SBS modified asphalt, 6-10 parts by weight of component regulator, 0.2-0.7 parts by weight of SBS structural regenerator, 0.1-0.3 parts by weight of compatibilizer, and 0.15-0.25 parts by weight of stabilizer. The component regulator is aromatic oil, the SBS structural regenerator is at least one of a polyepoxy group compound or a dioxazoline compound, the polyepoxy group compound is N,N,N,N,-tetraepoxypropyl-4,4-diaminodiphenylmethane, the dioxazoline compound is 2,2'-(1,3-phenylene)-dioxazoline, the compatibilizer is an acid anhydride compound, and the stabilizer is sulfur.

2. The high-performance recycled SBS modified bitumen according to claim 1, characterized in that... The kinematic viscosity of the aromatic oil at 100°C is 36.13 mm. 2 / s, moisture content 0.06%, density 0.9511g / cm³ 3 .

3. The high-performance recycled SBS modified bitumen according to claim 1, characterized in that... The acid anhydride compound is maleic anhydride or phthalic anhydride.

4. A method for preparing the high-performance recycled SBS modified asphalt according to any one of claims 1-3, characterized in that... The method includes the following steps: Step (1) Heat the aged SBS modified asphalt to 130~160℃, and add component regulators and compatibilizers while stirring continuously; Step (2) Add SBS structural regenerator at the same temperature and speed, and continue stirring; Step (3) Add the stabilizer at the same temperature and speed, and continue stirring; Step (4) Place the sample that has been stirred in step (3) in an environment of 120~140℃ for development. After development, cool it to room temperature to obtain high-performance recycled SBS modified asphalt.

5. The method for preparing high-performance recycled SBS modified asphalt according to claim 4, characterized in that... In step (1), the stirring speed is 1000~1200 r / min and the time is 3~5 min.

6. The method for preparing high-performance recycled SBS modified bitumen according to claim 4, characterized in that... In step (2), the stirring time is 15-20 minutes.

7. The method for preparing high-performance recycled SBS modified bitumen according to claim 4, characterized in that... In step (3), the stirring time is 10-15 minutes.

8. The method for preparing high-performance recycled SBS modified bitumen according to claim 4, characterized in that... In step (4), the development time is 20-40 minutes.

Citation Information

Patent Citations

  • SBS modified asphalt regenerant and preparation method thereof

    CN116178969A