A low-carbon alkali-activated marine silt composite and a preparation method thereof
By mixing marine silt with activated silica-alumina solid waste and an alkaline solution using a low-carbon alkaline activation method, a three-dimensional structure is generated, which solves the problem of marine silt resource utilization and achieves low-cost, low-pollution silt treatment and resource utilization.
Patent Information
- Application Number
- CN202410388491.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-01
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-04-01
AI Technical Summary
Existing technologies for treating marine silt suffer from high resource consumption, high pollution risk, and high cost. Furthermore, traditional binders cause serious environmental impacts, making it difficult to achieve efficient resource utilization of waste marine silt.
A low-carbon alkali activation method is adopted, which involves mixing marine silt with activated silica-alumina solid waste and an alkaline solution to form a low-carbon alkali activated marine silt complex. The alkaline solution is used to activate the reaction to generate a three-dimensional structure, thereby improving the mechanical properties and stability of the silt and realizing waste reuse.
It effectively reduces resource consumption and environmental pollution, improves the utilization rate of marine silt, reduces treatment costs, realizes the resource utilization of waste, and is superior to traditional methods in terms of strength and stability.
Smart Images

Figure CN118290089B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a green alkali-activated solidification method for marine silt, belonging to the fields of comprehensive utilization technology and environmental protection of waste marine silt. Background Technology
[0002] In recent years, to support the high-quality development of coastal cities, construction has been increasing in the southeastern coastal areas of China, especially for projects following land reclamation. However, during foundation construction, a large amount of marine silt with high water content is inevitably generated. This marine silt layer results in borehole soil in the area characterized by low bearing capacity, high initial water content, high liquid limit, and high compressibility. These disadvantages make the marine silt unsuitable for direct use in engineering construction. Improper disposal of this soil can pose a significant pollution risk, contaminating rivers, groundwater, and farmland. However, traditional management procedures, such as landfill and marine disposal, incur expensive site, transportation, and management costs. Therefore, it is essential to find more reasonable management methods for these waste soils.
[0003] Lime-based and cement-based materials are widely used as traditional binders in marine clay treatment. The calcium hydroxide in these materials exerts a cation exchange effect, causing clay particles to flocculate and agglomerate, resulting in rapid changes in plasticity, workability, and particle size distribution. Furthermore, calcium silicate hydrate (CSH) and calcium aluminate hydrate (CAH), produced by hydrogel reactions or cement hydration, effectively fill the micropores between soil particles, significantly improving the soil's mechanical strength.
[0004] This method allows for the reuse of large quantities of marine silt. However, the production of these two traditional materials inevitably consumes significant amounts of non-renewable resources and emits substantial amounts of greenhouse gases. Continued reliance on these materials for engineering projects will further exacerbate global warming. Current methods utilize large quantities of mixed curing agents or cement, with marine silt content not being a significant factor. Therefore, it is necessary to find more environmentally friendly alternatives, reduce cement usage, and further increase the marine silt content. This will also provide technical support for transforming marine clay into value-added products.
[0005] With the rapid pace of industrialization and urbanization, a large amount of non-renewable resources are being consumed quickly. At the same time, the infrastructure and construction industries are generating substantial amounts of waste. This not only leads to land, soil, and water degradation, causing serious environmental problems, but also hinders social progress due to the significantly increased cost of waste treatment, ultimately negatively impacting the balance between ecosystems and the economy. Utilizing solid waste resources while reusing abandoned marine silt is technically feasible and can ultimately achieve the goal of treating waste with waste. Summary of the Invention
[0006] To address the above problems, this invention proposes a green and low-cost method for solidifying marine silt. This invention combines marine silt with aluminosilicate waste, activates it with an alkaline solution, achieving waste reuse and achieving green and low-cost solidification without the need for additional additives. This invention combines the use of an alkaline activator with the utilization of solid waste, effectively improving the utilization rate of waste marine silt, promoting the comprehensive utilization of marine silt waste, and achieving the goal of treating waste with waste. To achieve the above-mentioned objectives, this invention provides the following technical solutions:
[0007] First aspect:
[0008] This invention provides a low-carbon alkali-activated marine silt composite, composed of component A and component B, wherein the mass ratio of component A to component B is 1:(0-2); wherein, based on 100 parts by weight, component A comprises: 85-95 parts marine silt, 5-10 parts activated aluminosilicate solid waste, and an alkaline solution with a solid-liquid ratio of 0.15-0.40; and based on 100 parts by weight, component B comprises 70-80 parts of the marine silt, 10-20 parts activated aluminosilicate solid waste, and 5-15 parts sea sand.
[0009] Preferably, the water content of the marine silt is 10%-80%, more preferably 30%-60%.
[0010] Preferably, the active silica-alumina solid waste includes fly ash and / or slag.
[0011] Preferably, the alkaline solution comprises a sodium hydroxide solution; the concentration of the alkaline solution is 3-8 mol / L, more preferably 3-6 mol / L.
[0012] Preferably, the active silica-alumina solid material includes at least one of fly ash, slag, and silicate cement.
[0013] This invention also provides a method for preparing a low-carbon alkali-activated marine silt complex, specifically comprising the following preparation steps:
[0014] (1) Preparation of component A: Marine silt, activated silica-alumina solid waste and alkaline solution are stirred according to the above mass parts to obtain component A;
[0015] (2) Preparation of component B: Marine silt, active aluminosilicate solids and sea sand are stirred according to the above mass proportions to obtain component B;
[0016] (3) Mix and stir the components A and B according to the above mass ratio.
[0017] Preferably, the stirring speed in step (1) is 300 rpm; the stirring time is 10-20 min.
[0018] Preferably, the stirring speed in step (2) is 300 rpm; the stirring time is 10-20 min.
[0019] Preferably, the stirring speed in step (3) is 300 rpm and the stirring time is 15 min.
[0020] The present invention also provides a low-carbon alkali-activated marine silt composite, which is prepared by the preparation method of the low-carbon alkali-activated marine silt composite as described above.
[0021] The present invention also provides the application of the low-carbon alkali-activated marine silt composite as described above as a material in the construction field.
[0022] The second aspect:
[0023] The marine silt described in this invention includes at least one of gravel, silt, and clay.
[0024] The average particle size of the gravel is 50 mm, the average particle size of the silt is 2–50 mm, and the average particle size of the clay is 2 mm.
[0025] The clay includes at least one of kaolinite, montmorillonite, diorite, and illite.
[0026] During the research process, this invention discovered that: marine mud is used as a raw material to provide a silicon-aluminum source for alkali-activated reaction, and fly ash or slag is used as an active silicon source. With the addition of an alkaline activator, alkali activation occurs. After the highly active silicon and aluminum elements in the slag dissolve in water, they undergo hydrolysis and polymerization reactions, finally generating a three-dimensional structure with silicon-aluminum tetrahedra as the basic unit. Furthermore, unreacted silicon, aluminates, and polymers will fill the gaps, thereby improving the mechanical properties of the product.
[0027] This invention has found that the curing time can be controlled by adjusting the concentration of NaOH.
[0028] Based on common knowledge in the field, the above-mentioned preferred conditions can be combined arbitrarily to obtain various preferred embodiments of the present invention.
[0029] The reagents and raw materials used in this invention are all commercially available.
[0030] Compared with the prior art, the beneficial effects of the present invention include:
[0031] 1. The curing agent of this invention contains mineral powder waste residue, which consumes a large amount of solid waste and realizes the resource utilization of waste residue, achieving the effect of treating waste with waste and greatly reducing the cost of marine silt disposal. This invention can effectively replace the traditional cement curing method, directly using the method of this invention to stimulate the mixing of marine silt for on-site utilization such as backfilling, thus realizing the resource utilization of marine silt and solving the problems of excavation, transportation and stockpiling of marine silt, reducing land occupation and environmental pollution.
[0032] 2. This invention can effectively save resources by using solid waste to replace traditional materials such as stone, cement, and complex curing agents, further reducing costs and realizing waste reuse. This invention uses an alkali activation method to solidify marine silt. Compared with traditional cement, it has high solidification strength, low heat of hydration, and the setting time can be controlled within the applicable strength range by adjusting the alkali activator, making it more suitable for large-scale on-site marine silt treatment.
[0033] 3. Compared with traditional solidification methods, the alkali-activated solidification method of this invention can effectively solidify and stabilize heavy metals, and the leaching concentration of heavy metals after solidification is greatly reduced, protecting the environment and reducing secondary pollution. At the same time, this invention achieves in-situ solidification and stabilization, effectively reducing construction costs, reducing construction steps, accelerating construction progress, and creating greater economic benefits. The marine silt solidification agent of this invention not only has a wide range of raw material sources, low cost, and simple production process, but also achieves high-efficiency comprehensive utilization by combining various solid wastes. Attached Figure Description
[0034] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.
[0035] Figure 1 Flowchart for the preparation of a complex for low-carbon alkali-activated marine silt;
[0036] Figure 2 This is a particle size distribution map of marine silt. Detailed Implementation
[0037] The physical properties of marine silt were tested, and the results are shown in Table 1.
[0038] Table 1
[0039]
[0040]
[0041]
[0042]
[0043] The particle size distribution curve is shown below. Figure 1 .
[0044] Example 1
[0045] (1) Preparation of component A: 90 parts of marine silt, 5 parts of slag and 5 parts of fly ash were added to a 5 mol / L sodium hydroxide solution with a solid-liquid ratio of 0.18 and stirred at 300 rpm for 10-20 min to obtain component A;
[0046] (2) Preparation of component B: 75 parts of marine silt, 5 parts of slag, 5 parts of fly ash, 5 parts of silicate cement and 10 parts of sea sand are added to water at a solid-liquid ratio of 0.3 and stirred at 300 rpm for 10-20 min to obtain component B;
[0047] (3) Mix component A and component B at a mass ratio of 1:1, stir at 300 rpm for 15 min, and then cure at room temperature for 10 days.
[0048] Example 2
[0049] (1) Preparation of component A: 90 parts of marine silt, 5 parts of slag and 5 parts of fly ash were added to a 5 mol / L sodium hydroxide solution with a solid-liquid ratio of 0.18 and stirred at 300 rpm for 10-20 min to obtain component A;
[0050] (2) Preparation of component B: 75 parts of marine silt, 5 parts of slag, 5 parts of fly ash, 5 parts of silicate cement and 10 parts of sea sand are added to water at a solid-liquid ratio of 0.3 and stirred at 300 rpm for 10-20 min to obtain component B;
[0051] (3) Mix component A and component B at a mass ratio of 1:2, stir at 300 rpm for 15 min, and then cure at room temperature for 10 days.
[0052] Example 3
[0053] (1) Preparation of component A: 85 parts of marine silt, 7.5 parts of slag, and 7.5 parts of fly ash were added to a 5 mol / L sodium hydroxide solution with a solid-liquid ratio of 0.18 and stirred at 300 rpm for 10-20 min to obtain component A;
[0054] (2) Preparation of component B: 75 parts of marine silt, 5 parts of slag, 5 parts of fly ash, 5 parts of silicate cement and 10 parts of sea sand are added to water at a solid-liquid ratio of 0.3 and stirred at 300 rpm for 10-20 min to obtain component B;
[0055] (3) Mix component A and component B at a mass ratio of 1:2, stir at 300 rpm for 15 min, and then cure at room temperature for 10 days.
[0056] Example 4
[0057] (1) Preparation of component A: 90 parts of marine silt, 5 parts of slag and 5 parts of fly ash were added to a 5 mol / L sodium hydroxide solution with a solid-liquid ratio of 0.18 and stirred at 300 rpm for 10-20 min to obtain component A;
[0058] (2) After stirring component A at 300 rpm for 15 min, it can be cured at room temperature for 10 days.
[0059] Comparative Example 1
[0060] Compared with Example 1, the only difference is that the mass ratio of component A to component B is 1:3, and all other conditions are the same. The specific operation is as follows:
[0061] (1) Preparation of component A: 90 parts of marine silt, 5 parts of slag and 5 parts of fly ash were added to a 5 mol / L sodium hydroxide solution with a solid-liquid ratio of 0.18 and stirred at 300 rpm for 10-20 min to obtain component A;
[0062] (2) Preparation of component B: 75 parts of marine silt, 5 parts of slag, 5 parts of fly ash, 5 parts of silicate cement and 10 parts of sea sand are added to water at a solid-liquid ratio of 0.3 and stirred at 300 rpm for 10-20 min to obtain component B;
[0063] (3) Mix component A and component B at a mass ratio of 1:3, stir at 300 rpm for 15 min, and then cure at room temperature for 10 days.
[0064] Comparative Example 2
[0065] Compared with Example 1, the only difference is the proportion of each component in component A; all other conditions are the same. The specific operation is as follows:
[0066] (1) Preparation of component A: 95 parts of marine silt, 2.5 parts of slag and 2.5 parts of fly ash were added to a 5 mol / L sodium hydroxide solution with a solid-liquid ratio of 0.18 and stirred at 300 rpm for 10-20 min to obtain component A;
[0067] (2) Preparation of component B: 75 parts of marine silt, 5 parts of slag, 5 parts of fly ash, 5 parts of silicate cement and 10 parts of sea sand are added to water at a solid-liquid ratio of 0.3 and stirred at 300 rpm for 10-20 min to obtain component B;
[0068] (3) Mix component A and component B at a mass ratio of 1:1, stir at 300 rpm for 15 min, and then cure at room temperature for 10 days.
[0069] Comparative Example 3
[0070] Compared with Example 1, the only difference is the solid-liquid ratio of sodium hydroxide added in component A; all other conditions are the same. The specific operation is as follows:
[0071] (1) Preparation of component A: 90 parts of marine silt, 5 parts of slag and 5 parts of fly ash were added to a 5 mol / L sodium hydroxide solution with a solid-liquid ratio of 0.6 and stirred at 300 rpm for 10-20 min to obtain component A;
[0072] (2) Preparation of component B: 75 parts of marine silt, 5 parts of slag, 5 parts of fly ash, 5 parts of silicate cement and 10 parts of sea sand are added to water at a solid-liquid ratio of 0.3 and stirred at 300 rpm for 10-20 min to obtain component B;
[0073] (3) Mix component A and component B at a mass ratio of 1:1, stir at 300 rpm for 15 min, and then cure at room temperature for 10 days.
[0074] Comparative Example 4
[0075] 75 parts marine silt, 15 parts silicate cement and 10 parts sea sand were added to water at a solid-liquid ratio of 0.3 and stirred at 300 rpm for 10-20 minutes to obtain the traditional OPC composition.
[0076] Example 1
[0077] Heavy metal pollution testing and assessment:
[0078] To assess the potential environmental impact of marine silt, this invention determines the leaching of heavy metals according to the People's Republic of China Environmental Protection Standard HJ557-2010 "Leaching Toxicity of Solid Waste - Horizontal Oscillation Method". Ceramic granules were dried, crushed, and cut, then passed through a 3mm sieve. Using pure water as the extraction solvent, pure water and the sample prepared in Example 1 were added to a beaker at a liquid-to-solid ratio of 10:1. The beaker was sealed with sealing film and fixed on a constant-temperature horizontal oscillator. The mixture was oscillated at a frequency of 110 ± 10 times / min for 8 hours at room temperature, followed by 16 hours of settling. The leachate was filtered through a 0.45mm filter membrane and collected, then stored at 0–4℃ for analysis. The leaching concentration of heavy metal elements was analyzed using inductively coupled plasma mass spectrometry (ICP-MS). The results were compared with the soil background control values GB36600-2018 (Class I Construction Land) and the US EPA standards. The leaching of heavy metals in untreated and treated marine silt (MM) was studied at 0 and 7 days, and the results are shown in Table 2.
[0079] Table 2
[0080]
[0081]
[0082] The NaOH solution in Example 1 was adjusted, where 3M represents a NaOH concentration of 3 mol / L; 6M represents a NaOH concentration of 6 mol / L; and 8M represents a NaOH concentration of 8 mol / L.
[0083] According to Table 2, all results meet the requirements and are lower than the maximum value required by the specification.
[0084] Therefore, it can be seen that the alkali-activated solidification method of the present invention can effectively solidify and stabilize heavy metals in marine silt. After solidification, the leaching concentration of heavy metals is greatly reduced. Moreover, even when the specific component requirements of the present invention are not met in Comparative Examples 1 to 3, the alkali-activated solidification method of the present invention can still meet the environmental requirements.
[0085] Example 2
[0086] 1. Curing time test:
[0087] In the initial experimental phase, curing time tests were conducted on Example 1 and Comparative Example 4, recording the curing process between initial and final setting. The degree of curing was compared by applying local pressure. The applied surface was 1 cm. 2 The pressure was applied at 1N, 2N and 3N respectively. When the pressure mark appeared on the surface (greater than 0.5mm from the surface), it could be defined as soft, moderate and hard (L, M and H) according to the applied pressure. The results are shown in Table 3.
[0088] Table 3 Hardening Time
[0089] Hardening time (days) 1 2 3 4 5 6 7 Comparative Example 4 H - - - - - H Example 1 (8M) H - - - - - H Example 1 (6M) M H - - - - H Example 1 (3M) M M H - - - H
[0090] *L: Soft, M, Medium, H, Hard
[0091] To investigate the hardening time of low-carbon alkali-activated marine silt composites, the NaOH solution in Example 1 was adjusted, where 3M represents a NaOH concentration of 3 mol / L; 6M represents a NaOH concentration of 6 mol / L; and 8M represents a NaOH concentration of 8 mol / L.
[0092] As can be seen from Table 3, Comparative Example 4, using the traditional cement curing method, began to harden on the first day. However, Example 1, utilizing the slag alkali-activated method of this invention, achieved hardening on the first day at a NaOH concentration of 8 mol / L, on the second day at 6 mol / L, and on the third day at 3 mol / L, effectively controlling the hardening time of the low-carbon alkali-activated marine silt composite.
[0093] During the research process, this invention hypothesized that the strength development of marine silt solidified using traditional methods in Comparative Example 4 was related to the reaction-generated chain-like CSH or CAH gel. The basic elements for gel formation are CaO, SiO2, and AlO3, with CaO provided by the solidifying agent being crucial for the green treatment of marine silt. However, this invention differs from traditional solidification methods. The alkali-activated solidifying agent primarily provides Na2O, which reacts with the silicon and aluminum elements in the marine silt and active aluminosilicate materials to form a three-dimensional NASH gel through silicon-aluminosilicate tetrahedra. This allows for effective control of the solidification time.
[0094] 2. Mechanical property testing:
[0095] We selected small specimens from Examples 1-3 and Comparative Examples 1-3 to conduct simple unconfined compressive strength (UCS) tests, and the specific results are shown in Table 4.
[0096] Table 4 Compressive Strength
[0097] Serial Number 14d compressive strength Example 1 2.713MPa Example 2 2.135MPa Example 3 2.251MPa Example 4 2.345MPa Comparative Example 1 1.659MPa Comparative Example 2 1.583MPa Comparative Example 3 0.828MPa
[0098] It can be seen that the compressive strength of Examples 1 to 4 of the present invention is significantly higher than that of Comparative Examples 1 to 3, especially Example 1, whose compressive strength (14d) can reach 2.713 MPa; while Comparative Example 3 has the worst mechanical properties, which is presumably due to the addition of excessive sodium hydroxide, thus affecting the compressive strength of the final product.
[0099] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A complex for activating marine silt with low carbon alkali, characterized in that, It consists of component A and component B, wherein the mass ratio of component A to component B is 1:(1-2); wherein, based on 100 parts by weight, component A comprises: 90 parts marine silt, 10 parts activated aluminosilicate solid waste, and an alkaline solution with a solid-liquid ratio of 0.15-0.40; and based on 100 parts by weight, component B comprises: 75 parts of the marine silt, 15 parts activated aluminosilicate solid waste, 10 parts sea sand, and water with a solid-liquid ratio of 0.15-0.
40. The water content of the marine silt is 10%-80%, and the particle size of the marine silt is 40-400 μm; The alkaline solution includes a sodium hydroxide solution; The active silica-alumina solid waste includes fly ash and / or slag; The active silica-alumina solid material includes at least one of fly ash, slag, and silicate cement.
2. The low-carbon alkali-activated marine silt composite as described in claim 1, characterized in that, The concentration of the alkaline solution is 3–8 mol / L.
3. A method for preparing a low-carbon alkali-activated marine silt composite as described in any one of claims 1 to 2, characterized in that, The specific preparation steps are as follows: (1) Preparation of component A: Marine silt, activated silica-alumina solid waste and alkaline solution are stirred according to the above mass parts to obtain component A; (2) Preparation of component B: Marine silt, active aluminosilicate solids, sea sand and water are stirred according to the above mass proportions to obtain component B; (3) Mix component A and component B according to the above mass ratio and then cure at room temperature for 7 to 14 days.
4. The method for preparing the low-carbon alkali-activated marine silt composite as described in claim 3, characterized in that, The stirring speed in step (1) is 300 rpm; the stirring time is 10-20 min.
5. The method for preparing the low-carbon alkali-activated marine silt composite as described in claim 3, characterized in that, In step (2), the stirring speed is 300 rpm and the stirring time is 10-20 min.
6. The method for preparing the low-carbon alkali-activated marine silt composite as described in claim 3, characterized in that, In step (3), the stirring speed is 300 rpm and the stirring time is 5-15 min.
7. The application of the low-carbon alkali-activated marine silt composite as described in any one of claims 1 to 2 as an in-situ backfill material in construction engineering.
Citation Information
Patent Citations
Curing agent for soft soil and application thereof
CN102153326A
Stabilized soil applicable to intertidal zone sludge stable layer
CN103553520A