A method for deeply separating arsenic and antimony from high-arsenic fume by using waste acid-phosphoric acid mixed acid

By leaching high-arsenic flue dust with a mixture of waste acid and phosphoric acid, and by controlling the reaction conditions, the problem of poor arsenic-antimony separation was solved. This achieved efficient and economical arsenic-antimony separation and waste acid treatment, resulting in high-purity antimony phosphate products and improving the environmental friendliness and economy of the process.

CN118291768BActive Publication Date: 2026-11-24JIANGXI UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410421380.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-09
Publication Date
2026-11-24
Estimated Expiration
2044-04-09

AI Technical Summary

Technical Problem

Existing technologies for treating high-arsenic fumes and smelting waste acid suffer from problems such as poor arsenic-antimony separation, long operation processes, equipment corrosion, high acid consumption, and poor working conditions for workers, making it difficult to achieve efficient and economical arsenic-antimony separation and waste acid treatment.

Method used

Arsenic-containing flue dust was leached using a mixture of polluted acid and phosphoric acid. By controlling the ratio of polluted acid to phosphoric acid, temperature, and liquid-solid ratio, deep separation of arsenic and antimony was achieved. Subsequently, the product was separated by stirring and centrifugation in a high-concentration phosphoric acid solution to obtain high-purity antimony phosphate product, and the separation liquid was recycled.

Benefits of technology

This method achieves efficient deep separation of arsenic and antimony, yields high-purity antimony phosphate products, reduces acid consumption, improves the working environment for workers, and realizes the high-value utilization of valuable metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118291768B_ABST
    Figure CN118291768B_ABST
Patent Text Reader

Abstract

This invention discloses a method for deep separation of arsenic and antimony from high-arsenic flue dust using a mixed acid-phosphoric acid solution. The method involves leaching the high-arsenic flue dust with the mixed acid to separate arsenic and antimony, yielding a primary antimony phosphate product and an arsenic-containing solution. The obtained primary antimony phosphate product is added to a high-concentration phosphoric acid solution, thoroughly stirred, and centrifuged to obtain a high-purity antimony phosphate product. The separation liquid is recycled. Based on the concept of "waste-to-waste," this invention achieves the synergistic treatment of high-arsenic flue dust and waste acid, while simultaneously achieving deep separation of arsenic and antimony from the high-arsenic flue dust. This invention is simple to operate, effectively reduces processing costs, and the final high-purity antimony phosphate product can be sold externally. The separation liquid is returned to the process flow, and the arsenic-containing solution is recycled, realizing the comprehensive recovery and utilization of arsenic and antimony resources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of non-ferrous metallurgical technology, specifically to a method for deep separation of arsenic and antimony from high-arsenic flue dust using a mixture of polluted acid and phosphoric acid. Background Technology

[0002] Arsenic is a common impurity element found in sulfide ores containing metals such as copper, lead, and zinc. Although most of the arsenic can be separated through mineral processing, it inevitably enters the smelting system. Due to its high volatility, arsenic accumulates in flue dust or flue gas scrubbing liquid, forming typical arsenic-containing materials such as high-arsenic flue dust and smelting waste acid. These arsenic-containing materials exhibit highly variable composition and contain a certain amount of valuable metals in addition to arsenic, possessing significant economic value. However, their high arsenic content makes processing extremely challenging and has long been a problem for the non-ferrous metals industry.

[0003] Currently, the main methods for treating high-arsenic flue dust are pyrometallurgical and hydrometallurgical processes. Pyrometallurgical processes offer the advantage of a short process flow, but the separation of arsenic and antimony is poor. Therefore, hydrometallurgical processes are the mainstream technology for treating high-arsenic flue dust. The core of hydrometallurgical treatment of high-arsenic flue dust is the selective leaching of arsenic and antimony. To this end, engineers have developed water leaching, alkaline leaching, and acid leaching methods for treating high-arsenic flue dust. Although water leaching can achieve selective arsenic leaching, it suffers from a low arsenic leaching rate. Alkaline leaching can achieve better separation of arsenic and antimony, but its high alkali consumption and cost make it difficult to apply industrially. Acid leaching utilizes various acid solutions, such as hydrochloric acid, sulfuric acid, and nitric acid, with the addition of various reducing agents or oxidizing agents to achieve simultaneous or separate leaching of arsenic and antimony from high-arsenic flue dust. This process has the advantages of a short process flow and low cost. For example, the method disclosed in CN107502753A uses sulfuric acid, hydrochloric acid, or a mixture of both as leaching agents to achieve an arsenic leaching rate of 80-95% in the flue dust. The method disclosed in CN106591586A uses recycled washing waste acid as a leaching agent to leach white dust, achieving an arsenic leaching rate of greater than 95%. The method disclosed in CN114574716A involves preliminary arsenic removal through oxidative acid leaching of antimony-containing high-arsenic flue dust in a sulfuric acid system, ensuring complete leaching of arsenic trioxide and soluble arsenate phases from the flue dust, while antimony remains in the acid leaching residue without leaching. Subsequently, sodium sulfide alkaline leaching further removes arsenic and leaches antimony, causing most of the arsenic and antimony in the acid leaching residue to leach into the solution. Reducing aluminum powder replaces the antimony in the solution, forming metallic antimony, thus achieving the separation of arsenic and antimony in the flue dust.

[0004] However, most acid leaching processes have poor arsenic and antimony separation effects and have disadvantages such as excessively long operation process, equipment corrosion, large acid consumption, and poor working environment for workers.

[0005] The disposal of waste acid from smelting is currently quite challenging. Traditional non-ferrous metal smelting processes generate large amounts of waste acid, containing 150–200 g / L of sulfuric acid, 0.5–1.5 g / L of fluorine, and 0.3–2 g / L of arsenic. Enterprises primarily use processes such as sulfide precipitation and lime-iron salt methods to treat this waste acid. While these processes can stabilize arsenic, the acidity is too high, requiring neutralization before treatment, thus consuming large amounts of alkali. Effective disposal of waste acid is crucial for achieving clean and stable production in non-ferrous metal smelting. Summary of the Invention

[0006] This invention relates to a method for deep separation of arsenic and antimony from high-arsenic flue dust using a mixture of polluted acid and phosphoric acid, thereby achieving the goal of deep separation of arsenic and antimony from high-antimony flue dust and realizing the resource utilization of arsenic.

[0007] To achieve the above objectives, this invention discloses a method for deep separation of arsenic and antimony from high-arsenic flue gas using a mixture of polluted acid and phosphoric acid, comprising the following steps:

[0008] 1) Use a mixture of waste acid and phosphoric acid to leach high-arsenic flue dust to separate arsenic and antimony, and obtain primary antimony phosphate product and arsenic-containing solution;

[0009] 2) The obtained primary antimony phosphate product is added to a high-concentration phosphoric acid solution, stirred thoroughly, and centrifuged to obtain a high-purity antimony phosphate product. The separation liquid is recycled.

[0010] Preferably, in the mixed acid-phosphoric acid mixture, the waste acid is various types of smelting waste acid, and the phosphoric acid is a pure phosphoric acid solution or a phosphate solution.

[0011] Preferably, the total sulfuric acid concentration in the waste acid-phosphoric acid mixture is 0.5 mol / L to 7 mol / L, and the phosphate ion concentration is 0.4 to 5 mol / L.

[0012] Preferably, the conditions in step 1) are: the liquid-solid ratio of high arsenic dust to polluted acid-phosphoric acid mixture is 10:1 to 50:1, the reaction temperature is 30 to 90°C, and the leaching time is 1 to 5 hours.

[0013] Preferably, the conditions in step 2) are: the phosphoric acid concentration in the high-concentration phosphoric acid solution is 4-10 mol / L, and the reaction temperature is 30-90℃.

[0014] The above technical solution can efficiently separate arsenic and antimony from high-arsenic flue dust, and obtain high-purity antimony phosphate product. The separation liquid can be reused.

[0015] The technical principle of this invention is as follows:

[0016] The waste acid contains a high concentration of sulfuric acid and a small amount of arsenic. The dissolution and leaching of As₂O₃ and Sb₂O₃ from high-arsenic flue dust requires a large amount of acid. Therefore, theoretically, high-arsenic flue dust can be directly leached with waste acid. However, during the leaching process, as the concentration of free As(III) in the solution gradually increases, As(III) readily reacts with Sb(III) or Sb₂O₃ to form low-solubility antimony arsenate or antimony arsenate solid solutions, thus affecting the separation of arsenic and antimony. Based on this principle, technicians often add Sb₂O₃ to remove arsenic during the purification process of copper electrolyte. Therefore, simply leaching high-arsenic flue dust with waste acid is not feasible. Furthermore, when phosphoric acid or phosphates are introduced into the waste acid system, PO₄²⁻… 3- Will with AsO3 3- or AsO2 - Together they participate in the reaction with Sb(III), or PO4 within the system 3- The concentration is much higher than that of AsO3 3- or AsO2 - At high concentrations, SbPO4 will preferentially form, rather than arsenic-antimony solid solutions. Simultaneously, the competition between arsenic and phosphorus promotes the leaching of arsenic from the flue dust, thus achieving deep separation of arsenic and antimony. Using a mixture of polluted acid and phosphoric acid can both consume excess acid in the polluted acid and achieve deep separation of arsenic and antimony in high-arsenic flue dust.

[0017] Based on the above technical ideas, the inventors proposed a method for deep separation of arsenic and antimony from high-arsenic flue dust using a mixture of polluted acid and phosphoric acid.

[0018] The present invention has the following beneficial effects:

[0019] This invention utilizes the raw material characteristics of high-arsenic fume and waste acid, based on the concept of "using waste to treat waste," to not only solve the environmental protection problems of treating high-arsenic fume and waste acid, but also realize the high-value utilization of valuable metals. Attached Figure Description

[0020] Figure 1 This is a schematic flowchart of a method for deep separation of arsenic and antimony from high-arsenic flue dust using a mixture of polluted acid and phosphoric acid, as proposed in this invention.

[0021] Figure 2 The effect of the ratio of polluted acid to phosphoric acid on the separation efficiency of arsenic in high-arsenic flue dust (a) and the effect on the separation efficiency of antimony (b);

[0022] Figure 3 XRD patterns of primary antimony phosphate products obtained under different waste acid-phosphoric acid ratios;

[0023] Figure 4 The SEM-EDS spectrum of the primary antimony phosphate product obtained when the volume ratio of concentrated phosphoric acid to waste acid is 0.071.

[0024] Figure 5The effect of reaction temperature on the separation efficiency of arsenic in high-arsenic flue dust (a) and the effect on the separation efficiency of antimony (b);

[0025] Figure 6 XRD patterns of primary antimony phosphate products obtained at different reaction temperatures;

[0026] Figure 7 The image shows the SEM-EDS spectrum of the high-purity antimony phosphate product obtained at a reaction temperature of 90℃.

[0027] Figure 8 The effect of liquid-to-solid ratio on the separation efficiency of arsenic in high-arsenic flue dust (a) and the effect on the separation efficiency of antimony (b);

[0028] Figure 9 The XRD patterns of primary antimony phosphate products obtained under different liquid-to-solid ratios are shown. Detailed Implementation

[0029] The present invention will be further described below with reference to the accompanying drawings. It should be noted that the following embodiments are based on the present technical solution and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to these embodiments.

[0030] The content of major components in high-arsenic flue dust and polluted acid varies considerably. The samples in Examples 1-3 were all collected from a non-ferrous metal smelter in my country. The main components of the high-arsenic flue dust are shown in Table 1, and the main components of the polluted acid are shown in Table 2.

[0031] Table 1. Main components of high-arsenic flue dust

[0032]

[0033] Table 2 Main Components of Waste Acid

[0034]

[0035] Example 1:

[0036] Take 100g of high-arsenic flue dust and add it to a mixture of waste acid and phosphoric acid at a liquid-solid ratio of 30:1. Control the volume ratio of concentrated phosphoric acid to waste acid to be 0, 0.035, 0.071, 0.111, 0.154, and 0.2, respectively. The total sulfuric acid concentration is 0.721, 0.697, 0.673, 0.649, 0.625, and 0.601 mol / L, respectively, and the phosphate ion concentration is 0, 0.487, 0.973, 1.460, 1.947, and 2.433 mol / L, respectively. The reaction temperature is 90℃, and the mixture is stirred for 3 hours under normal pressure.

[0037] Three hours later, liquid samples were taken for analysis. The arsenic concentrations were 25.88 g / L, 32.68 g / L, 33.37 g / L, 32.80 g / L, 32.27 g / L, and 31.31 g / L, respectively, with arsenic leaching rates of 51.04%, 92.47%, 99.50%, 99.48%, 99.62%, and 97.39%. The antimony concentrations were 495.35 mg / L, 428.86 mg / L, 349.48 mg / L, 351.82 mg / L, 349.83 mg / L, and 339.46 mg / L, with antimony leaching rates of 7.29%, 6.31%, 5.14%, 5.18%, 5.15%, and 4.99%, respectively. It can be seen that within a certain range, the arsenic-antimony separation effect improves with the increase of the proportion of phosphoric acid in the system. For a comparison of results, please refer to [link to results]. Figure 2 and Figure 3 .

[0038] When the volume ratio of concentrated phosphoric acid to waste acid is 0.071, the resulting primary antimony phosphate product is shown in the SEM-EDS image below. Figure 4 As shown, the arsenic content is 1.30%. When placed in a 6 mol / L phosphoric acid solution and stirred thoroughly at 90°C, the arsenic content of the high-purity antimony phosphate product after the reaction is less than 0.35%.

[0039] Example 2:

[0040] Take 100g of high-arsenic flue dust and add it to a mixture of waste acid and phosphoric acid at a liquid-solid ratio of 30:1. The volume ratio of concentrated phosphoric acid to waste acid is 0.071. The total sulfuric acid concentration is 0.673mol / L and the phosphate ion concentration is 0.973mol / L. Control the reaction temperature at 30℃, 45℃, 60℃, 75℃ and 90℃ respectively, and stir for 3h under normal pressure.

[0041] Three hours later, liquid samples were taken for analysis. The arsenic concentrations were 17.52 g / L, 20.71 g / L, 26.38 g / L, 30.49 g / L, and 33.37 g / L, with arsenic leaching rates of 10.27%, 28.24%, 60.14%, 82.18%, and 99.50%, respectively. The antimony concentrations were 784.94 mg / L, 531.88 mg / L, 522.01 mg / L, 469.59 mg / L, and 349.48 mg / L, with antimony leaching rates of 11.55%, 7.83%, 7.68%, 6.82%, and 5.14%, respectively. It can be seen that the arsenic-antimony separation effect improves with increasing reaction temperature. For a comparison of results, please refer to [link to results]. Figure 5 and Figure 6 .

[0042] When the reaction temperature is 90℃, the resulting primary antimony phosphate product has an arsenic content of 1.30%. When placed in an 8 mol / L phosphoric acid solution and stirred thoroughly at 90℃, the high-purity antimony phosphate product after the reaction has an arsenic content of less than 0.1%. Figure 7 As shown.

[0043] Example 3:

[0044] Take 100g of high-arsenic flue dust and add it to a mixture of waste acid and phosphoric acid at a certain liquid-solid ratio. The volume ratio of concentrated phosphoric acid to waste acid is 0.071. The total sulfuric acid concentration of the waste acid-phosphoric acid mixture is 0.673mol / L and the phosphate ion concentration is 0.973mol / L. Control the liquid-solid ratios to be 10:1, 20:1, 30:1, 40:1 and 50:1 respectively. The reaction temperature is 90℃ and the mixture is stirred for 3h under normal pressure.

[0045] Three hours later, liquid samples were taken for analysis. The arsenic concentrations were 36.73 g / L, 39.91 g / L, 33.67 g / L, 29.00 g / L, and 26.35 g / L, with arsenic leaching rates of 39.47%, 90.88%, 99.50%, 99.90%, and 99.96%, respectively. The antimony concentrations were 959.51 mg / L, 509.74 mg / L, 349.48 mg / L, 303.56 mg / L, and 277.70 mg / L, with antimony leaching rates of 4.71%, 5.00%, 5.14%, 5.96%, and 6.81%, respectively. It can be seen that the arsenic-antimony separation effect improves with increasing liquid-to-solid ratio. For a comparison of results, please refer to [link to results]. Figure 8 and Figure 9 .

[0046] When the liquid-to-solid ratio is 50:1, the resulting primary antimony phosphate product has an arsenic content of 1.30%. When placed in a 4 mol / L phosphoric acid solution and stirred thoroughly at 90°C, the high-purity antimony phosphate product after the reaction has an arsenic content of less than 0.8%.

[0047] For those skilled in the art, various corresponding changes and modifications can be made based on the above technical solutions and concepts, and all such changes and modifications should be included within the protection scope of the claims of this invention.

Claims

1. A method for deep separation of arsenic and antimony from high-arsenic flue gas using a mixture of polluted acid and phosphoric acid, characterized in that, Includes the following steps: 1) High-arsenic flue dust is leached using a mixture of waste acid and phosphoric acid to separate arsenic and antimony, yielding a primary antimony phosphate product and an arsenic-containing solution. The total sulfuric acid concentration in the waste acid-phosphoric acid mixture is 0.5 mol / L~7 mol / L, and the phosphate ion concentration is 0.4~5 mol / L. 2) The obtained primary antimony phosphate product is added to a high-concentration phosphoric acid solution, stirred thoroughly, and centrifuged to obtain a high-purity antimony phosphate product. The separation liquid is recycled. The conditions in step 2) are: the phosphoric acid concentration in the high-concentration phosphoric acid solution is 4~10 mol / L, and the reaction temperature is 30~90 ℃.

2. The method for deep separation of arsenic and antimony from high-arsenic flue dust using a mixture of polluted acid and phosphoric acid as described in claim 1, characterized in that, In the aforementioned waste acid-phosphoric acid mixture, the waste acid is various types of smelting waste acid, and the phosphoric acid is pure phosphoric acid solution or phosphate solution.

3. The method for deep separation of arsenic and antimony from high-arsenic flue gas using a mixture of polluted acid and phosphoric acid as described in claim 1, characterized in that, The conditions in step 1) are: the liquid-solid ratio of high arsenic fume to polluted acid-phosphoric acid mixture is 10:1 to 50:1, the reaction temperature is 30 to 90 ℃, and the leaching time is 1 to 5 h.

Citation Information

Patent Citations

  • Method for recovering multiple kinds of metal from flue dust in copper smelting

    CN106591586A

  • Copper smelting white smoke acid leaching and extraction impurity removal method

    CN107502753A

  • Method for removing arsenic from antimony-containing high-arsenic soot and recovering valuable metal antimony

    CN114574716A

  • Treatment of ores or metallurgical by-products containing arsenic and antimony

    US4102976A