A method for manufacturing a niobium-containing austenitic heat-resistant stainless steel round pipe blank
By optimizing the metallurgical process and continuous casting parameters, the production problem of niobium-containing austenitic heat-resistant stainless steel round tube billets in ASME CODE CASE 2328-1 was solved, achieving high-quality and stable round tube billet manufacturing, which is suitable for the manufacturing of high-efficiency ultra-supercritical boiler components, and improving the yield and production efficiency.
Patent Information
- Application Number
- CN202410291971.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-14
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-03-14
AI Technical Summary
Existing technologies are difficult to stably produce ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel round tube billets, resulting in problems such as low yield, unstable quality, and low production efficiency. In particular, defects such as niobium precipitation, segregation, porosity, and cracks are prone to occur during continuous casting.
The process route of electric furnace or alloy melting furnace smelting, argon-oxygen furnace refining, LF furnace refining, continuous casting and hot rolling is adopted. By optimizing the deoxidation process and matching the continuous casting process parameters, high-quality ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel continuous casting billets are prepared, and these billets are rolled into round tube billets, replacing the traditional argon-oxygen furnace smelting and die casting steel ingot process.
It improves the quality stability and yield of materials, reduces the scrap rate, ensures the purity and thermoplasticity of round tube blanks, and is suitable for the manufacture of high-parameter boiler superheaters and reheaters, thus promoting industrial production.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of stainless steel production technology, specifically relating to a method for manufacturing a niobium-containing austenitic heat-resistant stainless steel round tube blank. Background Technology
[0002] The construction of low-energy-consumption ultra-supercritical units and the continuous improvement of their power generation ratio are important ways to make clean and efficient use of coal resources.
[0003] ASME CODE CASE 2328-1 is a new type of niobium-containing austenitic heat-resistant stainless steel developed based on the traditional austenitic heat-resistant steel TP304H (18Cr-8Ni). Its nominal composition is 0.08C-18Cr-9Ni-3Cu-0.40Nb-0.1N, and its name in GB5310-2008 is 10Cr18Ni9NbCu3BN. Due to its high creep strength and good resistance to steam corrosion, ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel is a key material for manufacturing pressure-bearing heat-receiving components such as superheaters and reheaters in high-efficiency ultra-supercritical boilers with steam parameters of 600–630℃. It is also currently the most widely used austenitic heat-resistant steel with the highest technical quality requirements.
[0004] Compared to traditional stainless steel, ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel contains a large amount of alloying elements such as Cr, Ni, Nb, Cu, and N. The variety of chemical elements and the narrow control over composition make production extremely difficult. Furthermore, due to the compositional control requirements of low silicon (Si≤0.3%) and low aluminum (Al: 0.003~0.03%), poor steel reduction can lead to high residual oxygen content, causing nozzle clogging in continuous casting and interrupting production. Furthermore, due to the high carbon (C: 0.07%–0.13%) and niobium (Nb: 0.30–0.60%) content in steel, and the low solubility of niobium in molten steel, a large number of coarse micron-sized niobium compounds precipitate in the melt during continuous casting as the temperature of the molten steel decreases. These large-sized niobium compounds cause severe segregation and porosity during the solidification process of the molten steel. The resulting billet has poor plasticity, uneven internal structure, and is prone to cracks and delamination defects, leading to a high scrap rate during subsequent rolling and pipe threading.
[0005] For the reasons mentioned above, only a very few steel mills are currently able to produce ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel round tube billets. The main process route is "argon-oxygen furnace smelting → die casting of steel ingots → ingot rolling or forging". The round tube billets produced by the die casting method have a low yield, and the rough tubes often have quality defects such as internal wall cracks and internal wall delamination during hot piercing, resulting in low yield, unstable quality, and low production efficiency. This directly restricts the industrial production of ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel round tube billets. Summary of the Invention
[0006] To address some or all of the technical problems existing in the prior art, the present invention provides a method for manufacturing a niobium-containing austenitic heat-resistant stainless steel round tube blank, comprising the following steps:
[0007] (1) Smelting in electric furnace or alloy melting furnace
[0008] According to the chemical composition requirements of niobium-containing austenitic heat-resistant stainless steel, scrap steel and alloy are used as smelting raw materials for batching. The batched scrap steel and alloy are added to an electric furnace or alloy melting furnace, and the scrap steel and alloy are heated by electricity to melt them, thus preparing the initial smelting mother liquor of niobium-containing austenitic heat-resistant stainless steel.
[0009] (2) Argon-oxygen furnace refining
[0010] The initial smelting mother liquor of niobium-containing austenitic heat-resistant stainless steel is added to an argon-oxygen furnace for refining. The carbon content at the end of the oxidation period is controlled to be ≤0.05%. During the oxidation period, alloys are added according to the composition control target of niobium-containing austenitic heat-resistant stainless steel. Aluminum is used as a reducing agent during the reduction period. The basicity of the reduction slag is controlled to be ≥2.0. The aluminum content in the molten steel is adjusted to 0.010~0.030%. The [O] content in the molten steel exiting the argon-oxygen furnace is controlled to be ≤20ppm.
[0011] (3) LF furnace refining
[0012] Under the condition of ensuring the fluidity of the slag surface, bottom blowing argon gas is used for stirring. The argon gas flow rate is controlled at 180-200 L / min, the stirring time is controlled at 8-15 min, and the steel liquid calming time is controlled at 10-20 min.
[0013] (4) Continuous casting
[0014] After refining, the molten steel is introduced into the tundish and continuously cast into round, square, or rectangular billets by the casting machine. The molten steel in the tundish is introduced into the crystallizer through a submerged entry nozzle. The continuous casting process parameters are controlled as follows: tundish superheat 30-65℃, tundish upper and lower nozzle diameter 30-50mm, submerged entry nozzle insertion depth 100-125mm, billet casting speed 0.80-1.00m / min, secondary cooling water ratio 0.15-0.30L / Kg, end electromagnetic stirring current intensity 280-600A, and end electromagnetic stirring frequency 3-8HZ.
[0015] (5) Heating of billet
[0016] The heating temperature is controlled at 1240~1280℃, and the heating time is controlled at 1.5~2min / mm based on the diameter of the round continuous casting billet or the side length of the cross section of the square or rectangular continuous casting billet.
[0017] (6) Hot-rolled round tube billet
[0018] The heated continuous casting billet is hot-rolled into a round tube billet in one heat. During the hot rolling process, the compression ratio is controlled at ≥6, the surface temperature of the initial rolling is controlled at 1100~1150℃, and the surface temperature of the hot rolling process and the final rolling is controlled at above 1000℃. The hot rolling is carried out in 5~13 passes, the deformation amount per pass is controlled at 8~15%, and the rolling speed is controlled at 1~1.2m / s.
[0019] Furthermore, in the above-mentioned method for manufacturing niobium-containing austenitic heat-resistant stainless steel round tube billets, between the continuous casting step and the billet heating step, a billet surface inspection / grinding step is also included. In the billet surface inspection / grinding step, defects on the billet surface and within 0.5 mm below the surface are ground, and the ratio of the grinding depth, width and length is controlled to be not less than 1:5:7.
[0020] Furthermore, in the above-mentioned method for manufacturing niobium-containing austenitic heat-resistant stainless steel round tube blanks, the niobium-containing austenitic heat-resistant stainless steel is ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel, and its chemical composition by mass percentage is: C 0.07~0.13%, Si≤0.30%, Mn≤1.00%, P≤0.035%, S≤0.010%, Cr 17.00~19.00%, Ni 8.50~10.50%, Mo 0.15~0.30%, Cu 2.50~3.50%, Nb 0.30~0.60%, N 0.05~0.15%, B 0.001~0.010%, Al 0.003~0.030%, with the remainder being Fe and unavoidable impurities.
[0021] Furthermore, in the above-mentioned method for manufacturing niobium-containing austenitic heat-resistant stainless steel round tube billets, the chemical composition of the molten steel is adjusted by mass percentage through LF furnace refining as follows: C 0.07~0.13%, Si≤0.30%, Mn≤1.00%, P≤0.035%, S≤0.010%, Cr 17.00~19.00%, Ni 8.50~10.50%, Mo 0.15~0.30%, Cu 2.50~3.50%, Nb 0.30~0.60%, N 0.05~0.15%, B 0.001~0.010%, Al 0.003~0.030%, [O]≤30ppm, with the remainder being Fe and unavoidable impurities.
[0022] Furthermore, in the above-mentioned method for manufacturing niobium-containing austenitic heat-resistant stainless steel round tube billets, the continuously cast billet obtained by the continuous casting step is a round continuously cast billet with a diameter of Φ240~350mm or a square or rectangular continuously cast billet with a cross-sectional side length of (200~300mm)×(200~300mm).
[0023] Furthermore, in the above-mentioned method for manufacturing niobium-containing austenitic heat-resistant stainless steel round tube billets, the proportion of the equiaxed crystal zone in the core of the continuously cast billet obtained by the continuous casting step is more than 20% of the cross-sectional area of the continuously cast billet, and the proportion of the central porosity and shrinkage cavity defect area is less than 5% of the cross-sectional area of the continuously cast billet.
[0024] Furthermore, in the above-mentioned method for manufacturing niobium-containing austenitic heat-resistant stainless steel round tube blanks, the round tube blanks obtained in the hot-rolled round tube blank step are round tube blanks with a diameter of 85 to 110 mm.
[0025] Furthermore, in the above-mentioned method for manufacturing niobium-containing austenitic heat-resistant stainless steel round tube blanks, the cross-sectional grain size of the round tube blank obtained by the hot-rolled round tube blank step is grade 5 to 8, and the grain size difference is within 2 grades.
[0026] The manufacturing method of niobium-containing austenitic heat-resistant stainless steel round tube billets of the present invention adopts the process route of "electric furnace or alloy melting furnace smelting → argon-oxygen furnace refining → LF furnace refining → continuous casting of square or round billets → billet heating → hot rolling of round tube billets". First, an ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel continuous casting billet is prepared. Then, this continuous casting billet is used as raw material to roll into ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel round tube billets. This method replaces the existing process of "argon-oxygen furnace smelting → die casting of steel ingots → ingot billet rolling or forging". It can stably prepare ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel round tube billets suitable for manufacturing pressure-bearing heat-receiving components such as superheaters and reheaters of high-efficiency ultra-supercritical boilers with steam parameters of 600-630℃. Compared with the prior art, the manufacturing method of niobium-containing austenitic heat-resistant stainless steel round tube billets of the present invention has the following advantages and beneficial effects:
[0027] (1) This invention, through reasonable optimization of the deoxidation process, matching of the continuous casting process, and key parameters such as billet heating and rolling, has developed a process method for producing ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel round tube billets. This method involves "smelting in an electric furnace or alloy melting furnace → refining in an argon-oxygen furnace → refining in an LF furnace → continuous casting of square or round billets → billet heating → hot rolling of round tube billets". This improves the material's quality stability, yield, and production efficiency. The resulting ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel round tube billets are suitable for manufacturing pressure-bearing and heat-receiving components such as boiler superheaters and reheaters for high-parameter, high-performance, large-capacity, and low-energy-consumption ultra-supercritical units. This promotes the industrial production of ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel products and provides technical support for the construction of ultra-supercritical units in my country.
[0028] (2) The method for manufacturing niobium-containing austenitic heat-resistant stainless steel round tube blanks of the present invention has significant economic benefits. Compared with the existing process of "argon-oxygen furnace smelting → die casting of steel ingots → steel ingot billet rolling or forging", the tube blank yield is increased by 12-15%, and the scrap rate of raw tubes in hot piercing is reduced by more than 10%.
[0029] (3) The steel has high purity and strong thermoplasticity. The total oxygen content is less than 30 ppm. The coarseness of each type of inclusion, including A (sulfides), B (oxides), C (silicates), and D (dot or spherical inclusions), is controlled within 2.0 level. The total amount of the nine types of inclusions is within 4 levels. The niobium-containing austenitic heat-resistant stainless steel round tube billet prepared in this way has a uniform structure. The grain size of the cross section of the round tube billet is controlled within 5 to 8 levels, and the grain size difference is controlled within 2 levels. The round tube billet does not need to be heat-treated in the later use.
[0030] (4) This invention ensures sufficient heat in the crystallizer and good slag formation by reasonably matching key continuous casting process parameters such as tundish superheat, tundish upper and lower nozzle diameters, and nozzle insertion depth, thereby stabilizing the crystallizer flow field and reducing the impact depth of the steel flow. By reasonably controlling key continuous casting process parameters such as billet casting speed and specific water volume, the initial solidified shell thickness of the billet is ensured, and the grain size of the fine grain layer on the surface of the billet and the width of the primary dendrites are controlled. By reasonably selecting the end electromagnetic stirring parameters, the generation of coarse columnar crystal regions in the billet is prevented, the proportion of the equiaxed crystal region in the core of the billet to the cross-sectional area of the billet is increased to more than 20%, and the proportion of the central loose and shrinkage cavity defect region to the cross-sectional area of the billet is reduced to less than 5%, thereby effectively improving the overall quality and performance of ASME CODECASE 2328-1 niobium-containing austenitic heat-resistant stainless steel round tube billets. Detailed Implementation
[0031] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0032] To improve quality stability, yield, and production efficiency, this invention provides a method for manufacturing niobium-containing austenitic heat-resistant stainless steel round tube billets. The process route is "smelting in an electric furnace or alloy melting furnace → refining in an argon-oxygen furnace → refining in an LF furnace → continuous casting of square or round billets → billet heating → hot rolling of round tube billets". First, an ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel continuous casting billet is prepared. Then, the continuous casting billet is used as raw material to roll into ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel round tube billets. The chemical composition of the niobium-containing austenitic heat-resistant stainless steel of ASME CODE CASE 2328-1 involved in this invention, by mass percentage, is as follows: C 0.07-0.13%, Si≤0.30%, Mn≤1.00%, P≤0.035%, S≤0.010%, Cr 17.00-19.00%, Ni 8.50-10.50%, Mo 0.15-0.30%, Cu 2.50-3.50%, Nb 0.30-0.60%, N 0.05-0.15%, B 0.001-0.010%, Al 0.003-0.030%, with the remainder being Fe and unavoidable impurities. The overall technical concept of this invention is as follows: Based on the composition, solidification and hot working characteristics of niobium-containing austenitic heat-resistant stainless steel according to ASME CODE CASE 2328-1, by reasonably optimizing the converter deoxidation process and matching the continuous casting process parameters, the internal metallurgical quality of the billet is improved, and a manufacturing method for niobium-containing austenitic heat-resistant stainless steel round tube billets according to ASME CODE CASE 2328-1 is developed.
[0033] Specifically, the method for manufacturing a niobium-containing austenitic heat-resistant stainless steel round tube blank of the present invention includes the following steps:
[0034] (1) Smelting in electric furnace or alloy melting furnace
[0035] According to the chemical composition requirements of niobium-containing austenitic heat-resistant stainless steel, scrap steel and alloys are used as smelting raw materials for batching. The batched scrap steel and alloys are added to an electric furnace or alloy melting furnace, and electric heating is applied to melt the scrap steel and alloys so that the chemical composition of the molten steel enters the chemical composition control range, thus preparing the primary smelting mother liquor of niobium-containing austenitic heat-resistant stainless steel that meets the requirements of argon-oxygen furnace smelting.
[0036] The primary smelting mother liquor containing niobium austenitic heat-resistant stainless steel that meets the requirements of argon-oxygen furnace smelting is prepared through the smelting process of electric furnace or alloy melting furnace. In this process, it is particularly important to strictly control the content of Si, Cr and Ni to a certain range so that the primary smelting mother liquor meets the composition requirements for argon-oxygen furnace refining, thus creating conditions for subsequent argon-oxygen furnace smelting.
[0037] (2) Argon-oxygen furnace refining
[0038] The prepared niobium-containing austenitic heat-resistant stainless steel primary smelting mother liquor is added to an argon-oxygen furnace for refining. During the oxidation period of the argon-oxygen furnace, the oxygen blowing amount is strictly controlled to prevent over-blowing and ensure that the final carbon content is controlled to ≤0.05%. During the oxidation period, alloys are added according to the composition control target of the niobium-containing austenitic heat-resistant stainless steel, and the composition is gradually adjusted to the internal control range. During the reduction period, aluminum is used as a reducing agent, the basicity of the reduction slag is controlled to ≥2.0, and the aluminum content in the molten steel is adjusted to 0.010~0.030%. The [O] content in the molten steel exiting the argon-oxygen furnace is controlled to ≤20ppm to reduce the amount of oxides formed and avoid subsequent continuous casting nozzle nodule formation.
[0039] By using the argon-oxygen furnace refining process, while ensuring that all chemical components in the steel are within the internal control range, the total oxygen content in the steel is reduced to below 20 ppm by optimizing the deoxidation process. The coarseness of inclusions of type A (sulfides), type B (oxides), type C (silicates), and type D (dot-like or spherical inclusions) is controlled to be within level 2.0, and the total amount of the nine types of inclusions is controlled to be within level 4, thereby improving the purity of the steel and enhancing the thermoplasticity of the material.
[0040] (3) LF furnace refining
[0041] Based on the incoming temperature and composition, fine-tune the temperature and composition to the target requirements. While ensuring slag surface fluidity, use bottom-blown argon for stirring, controlling the argon flow rate at 180–200 L / min and the stirring time at 8–15 min to ensure uniform steel composition and temperature. After LF refining, control the steel's settling time at 10–20 min to promote the full flotation and removal of inclusions. Through LF furnace refining, adjust the chemical composition of the molten steel by mass percentage as follows: C 0.07–0.13%, Si≤0.30%, Mn≤1.00%, P≤0.035%, S≤0.010%, Cr 17.00–19.00%, Ni 8.50–10.50%, Mo 0.15–0.30%, Cu 2.50–3.50%, Nb 0.30–0.60%, N 0.05–0.15%, B 0.001–0.010%, Al 0.003–0.030%, [O] ≤30ppm, the remainder being Fe and unavoidable impurities.
[0042] Refining in an LF furnace further improves the purity of the steel and provides assurance for continuous casting.
[0043] (4) Continuous casting
[0044] After LF refining, the molten steel is introduced into the tundish and continuously cast into a round continuous casting billet with a diameter of Φ240~350mm or a square or rectangular continuous casting billet with a cross-sectional side length of (200~300mm)×(200~300mm). The molten steel in the tundish is introduced into the crystallizer through a submerged entry nozzle. The continuous casting process parameters are controlled as follows: tundish superheat 30~65℃, tundish upper and lower nozzle diameter 30~50mm, submerged entry nozzle insertion depth 100~125mm, billet casting speed 0.80~1.00m / min, secondary cooling water ratio 0.15~0.30L / Kg, end electromagnetic stirring current intensity 280~600A, and end electromagnetic stirring frequency 3~8HZ.
[0045] (5) Heating of billet
[0046] The continuous casting billet is heated at a temperature of 1240–1280℃. The heating time is controlled at 1.5–2 min / mm based on the diameter of the round continuous casting billet or the side length of the cross-section of the square or rectangular continuous casting billet, in order to ensure that the continuous casting billet is heated evenly and has the best thermoplasticity.
[0047] (6) Hot-rolled round tube billet
[0048] The heated continuous casting billet is hot-rolled into a round tube billet with a diameter of Φ85~110mm in one heat. During the hot rolling process, the compression ratio is controlled at ≥6, the surface temperature at the beginning of the rolling process is controlled at 1100~1150℃, and the surface temperature at the end of the hot rolling process is controlled at above 1000℃. The hot rolling is carried out in 5~13 passes, the deformation per pass is controlled at 8~15%, and the rolling speed is controlled at 1~1.2m / s.
[0049] Furthermore, between the aforementioned continuous casting step and billet heating step, there is also a billet surface inspection / grinding step. In the billet surface inspection / grinding step, the surface of the continuously cast billet is inspected, and the billet surface is required to be free of defects such as slag inclusion, pits, and cracks. Defects on the billet surface and within 0.5 mm below the surface are ground, and the ratio of the grinding depth, width and length is controlled to be not less than 1:5:7.
[0050] Therefore, by using the manufacturing method of the niobium-containing austenitic heat-resistant stainless steel round tube billet of the present invention, an ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel continuous casting billet is first prepared, and then the continuous casting billet is used as raw material to roll into an ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel round tube billet. The ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel round tube billet finally manufactured can be used to manufacture pressure-bearing heat-receiving components such as boiler superheaters and reheaters of ultra-supercritical units with high parameters, high performance, large capacity, and low energy consumption.
[0051] The following describes in detail the specific implementation of the method for manufacturing the niobium-containing austenitic heat-resistant stainless steel round tube blank of the present invention with reference to the embodiments. However, the specific implementation of the present invention is not limited to the following embodiments.
[0052] Example 1
[0053] Example 1 of this invention employs a process route of "smelting in an electric furnace or alloy melting furnace → refining in an argon-oxygen furnace → refining in an LF furnace → continuous casting of square or round billets → billet heating → hot-rolled round tube billets" to produce niobium-containing austenitic heat-resistant stainless steel round tube billets according to ASME CODE CASE 2328-1. The manufactured round tube billet has a specification of Φ110mm. The specific implementation of the manufacturing method of niobium-containing austenitic heat-resistant stainless steel round tube billets in Example 1 is as follows:
[0054] (1) Smelting in electric furnace or alloy melting furnace
[0055] According to the chemical composition requirements of niobium-containing austenitic heat-resistant stainless steel, scrap steel and alloys are used as smelting raw materials for batching. The batched scrap steel and alloys are added to an electric furnace or alloy melting furnace, and electric heating is used to melt the scrap steel and alloys to prepare the primary smelting mother liquor of niobium-containing austenitic heat-resistant stainless steel that meets the requirements of argon-oxygen furnace smelting.
[0056] (2) Argon-oxygen furnace refining
[0057] The prepared niobium-containing austenitic heat-resistant stainless steel primary smelting mother liquor was added to an argon-oxygen furnace for refining. The carbon content at the end of the oxidation period in the argon-oxygen furnace was controlled at 0.04%. During the reduction period, all-aluminum deoxidation was used, the basicity of the reduction slag was controlled at 2.1, the aluminum content at the outlet was adjusted to 0.011%, and the [O] content in the molten steel exiting the argon-oxygen furnace was 17 ppm.
[0058] (3) LF furnace refining
[0059] Under conditions of good slag surface fluidity in the ladle, argon gas was blown and stirred at the bottom of the ladle at a flow rate of 180 L / min for 8 min. The molten steel was then allowed to settle for 15 min. The chemical composition of the molten steel leaving the station was adjusted by mass percentage as follows: C 0.08%, Si 0.15%, Mn 0.73%, P 0.026%, S 0.001%, Cr 18.2%, Ni 8.90%, Mo 0.21%, Cu 2.92%, Nb 0.45%, N 0.11%, B 0.006%, Al 0.015%, [O] 28 ppm, with the remainder being Fe and unavoidable impurities.
[0060] (4) Continuous casting
[0061] After LF refining, the molten steel is introduced into the tundish and continuously cast into a square continuous casting billet with a cross-sectional side length of 240mm×240mm. The continuous casting process parameters are controlled as follows: tundish superheat 40℃, tundish upper and lower nozzle diameter 35mm, submerged entry nozzle insertion depth 110mm, billet casting speed 0.80~1.00m / min, specific water volume 0.20L / Kg, end electromagnetic stirring current intensity 350A, and end electromagnetic stirring frequency 5HZ.
[0062] (5) Heating of billet
[0063] The continuously cast billet is heated at a temperature of 1260℃ for 480 minutes.
[0064] (6) Hot-rolled round tube billet
[0065] A heated 240mm×240mm square billet is hot-rolled into a Φ110mm round tube billet in one pass. The compression ratio is 6, the initial rolling surface temperature is 1151℃, and the final rolling surface temperature is above 1023℃. The hot rolling is carried out in 7 passes, with a single pass deformation of 9% and a rolling speed of 1.1m / s.
[0066] Actual testing revealed that the ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel continuous casting billet, prepared using the manufacturing method of Example 1, exhibited an equiaxed grain region in the core accounting for 30% of the billet's cross-sectional area, and a central porosity and shrinkage cavity defect area accounting for less than 5% of the billet's cross-sectional area. The billet exhibited a uniform microstructure, high thermoplasticity, and was free of subcutaneous inclusions and surface cracks, demonstrating stable overall quality. Furthermore, the ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel round tube billet manufactured using this continuous casting billet showed a cross-sectional grain size of 6-7, with a uniform internal microstructure. During subsequent manufacturing of pressure-bearing heat-receiving components such as superheaters and reheaters for high-efficiency ultra-supercritical boilers with steam parameters of 600-630℃, no cracks or delamination defects were observed, and the scrap rate during rolling and tube threading was extremely low.
[0067] In summary, the manufacturing method of the niobium-containing austenitic heat-resistant stainless steel round tube billet of the present invention adopts the process route of "electric furnace or alloy melting furnace smelting → argon-oxygen furnace refining → LF furnace refining → continuous casting of square or round billets → billet heating → hot rolling of round tube billets". First, an ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel continuous casting billet is prepared. Then, this continuous casting billet is used as raw material to roll into ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel round tube billets. This method replaces the existing process of "argon-oxygen furnace smelting → ingot casting → ingot billet rolling or forging". It can stably prepare ASME CODE CASE billets suitable for manufacturing high-efficiency ultra-supercritical boiler superheaters, reheaters, and other pressure-bearing heat-receiving components with steam parameters of 600-630℃. 2328-1 Niobium-containing austenitic heat-resistant stainless steel round tube billet. Compared with the prior art, the manufacturing method of the niobium-containing austenitic heat-resistant stainless steel round tube billet of the present invention has the following advantages and beneficial effects:
[0068] (1) This invention, through reasonable optimization of the deoxidation process, matching of the continuous casting process, and key parameters such as billet heating and rolling, has developed a process method for producing ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel round tube billets. This method involves "smelting in an electric furnace or alloy melting furnace → refining in an argon-oxygen furnace → refining in an LF furnace → continuous casting of square or round billets → billet heating → hot rolling of round tube billets". This improves the material's quality stability, yield, and production efficiency. The resulting ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel round tube billets are suitable for manufacturing pressure-bearing and heat-receiving components such as boiler superheaters and reheaters for high-parameter, high-performance, large-capacity, and low-energy-consumption ultra-supercritical units. This promotes the industrial production of ASME CODE CASE 2328-1 niobium-containing austenitic heat-resistant stainless steel products and provides technical support for the construction of ultra-supercritical units in my country.
[0069] (2) The method for manufacturing niobium-containing austenitic heat-resistant stainless steel round tube blanks of the present invention has significant economic benefits. Compared with the existing process of "argon-oxygen furnace smelting → die casting of steel ingots → steel ingot billet rolling or forging", the tube blank yield is increased by 12-15%, and the scrap rate of raw tubes in hot piercing is reduced by more than 10%.
[0070] (3) The steel has high purity and strong thermoplasticity. The total oxygen content is less than 30 ppm. The coarseness of each type of inclusion, including A (sulfides), B (oxides), C (silicates), and D (dot or spherical inclusions), is controlled within 2.0 level. The total amount of the nine types of inclusions is within 4 levels. The niobium-containing austenitic heat-resistant stainless steel round tube billet prepared in this way has a uniform structure. The grain size of the cross section of the round tube billet is controlled within 5 to 8 levels, and the grain size difference is controlled within 2 levels. The round tube billet does not need to be heat-treated in the later use.
[0071] (4) This invention ensures sufficient heat in the crystallizer and good slag formation by reasonably matching key continuous casting process parameters such as tundish superheat, tundish upper and lower nozzle diameters, and nozzle insertion depth, thereby stabilizing the crystallizer flow field and reducing the impact depth of the steel flow. By reasonably controlling key continuous casting process parameters such as billet casting speed and specific water volume, the initial solidified shell thickness of the billet is ensured, and the grain size of the fine grain layer on the surface of the billet and the width of the primary dendrites are controlled. By reasonably selecting the end electromagnetic stirring parameters, the generation of coarse columnar crystal regions in the billet is prevented, the proportion of the equiaxed crystal region in the core of the billet to the cross-sectional area of the billet is increased to more than 20%, and the proportion of the central loose and shrinkage cavity defect region to the cross-sectional area of the billet is reduced to less than 5%, thereby effectively improving the overall quality and performance of ASME CODECASE 2328-1 niobium-containing austenitic heat-resistant stainless steel round tube billets.
[0072] It should be noted that, in this document, the term "comprising" or any other variation thereof is intended to cover non-exclusive inclusion, such that an article or device that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such an article or device.
[0073] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for manufacturing a niobium-containing austenitic heat-resistant stainless steel round tube blank, characterized in that, The chemical composition of the niobium-containing austenitic heat-resistant stainless steel, by mass percentage, is: C 0.07~0.13%, Si≤0.30%, Mn≤1.00%, P≤0.035%, S≤0.010%, Cr 17.00~19.00%, Ni 8.50~10.50%, Mo 0.15~0.30%, Cu 2.50~3.50%, Nb 0.30~0.60%, N 0.05~0.15%, B 0.001~0.010%, Al 0.003~0.030%, with the remainder being Fe and unavoidable impurities. The method includes the following steps: (1) Smelting in electric furnace or alloy melting furnace According to the chemical composition requirements of niobium-containing austenitic heat-resistant stainless steel, scrap steel and alloy are used as smelting raw materials for batching. The batched scrap steel and alloy are added to an electric furnace or alloy melting furnace, and the scrap steel and alloy are heated by electricity to melt them, thus preparing the initial smelting mother liquor of niobium-containing austenitic heat-resistant stainless steel. (2) Argon-oxygen furnace refining The initial smelting mother liquor of niobium-containing austenitic heat-resistant stainless steel is added to an argon-oxygen furnace for refining. The carbon content at the end of the oxidation period is controlled to be ≤0.05%. During the oxidation period, alloys are added according to the composition control target of niobium-containing austenitic heat-resistant stainless steel. Aluminum is used as a reducing agent during the reduction period. The basicity of the reduction slag is controlled to be ≥2.
0. The aluminum content in the molten steel is adjusted to 0.010~0.030%. The [O] content in the molten steel exiting the argon-oxygen furnace is controlled to be ≤20ppm. (3) LF furnace refining Under the condition of ensuring the fluidity of the slag surface, bottom blowing argon gas is used for stirring, with the argon gas flow rate controlled at 180~200L / min, the stirring time controlled at 8~15min, and the steel liquid calming time controlled at 10~20min. (4) Continuous casting After LF refining, the molten steel is introduced into the tundish and continuously cast into round, square, or rectangular billets by the casting machine. The molten steel in the tundish is introduced into the crystallizer through a submerged entry nozzle. The continuous casting process parameters are controlled as follows: tundish superheat 30~65℃, tundish upper and lower nozzle diameter 30~50mm, submerged entry nozzle insertion depth 100~125mm, billet casting speed 0.80~1.00m / min, secondary cooling water ratio 0.15~0.30L / Kg, end electromagnetic stirring current intensity 280~600A, and end electromagnetic stirring frequency 3~8HZ. (5) Heating of the billet The heating temperature is controlled at 1240~1280℃, and the heating time is controlled at 1.5~2min / mm based on the diameter of the round continuous casting billet or the side length of the cross section of the square or rectangular continuous casting billet. (6) Hot-rolled round tube billet The heated continuous casting billet is hot-rolled into a round tube billet in one heat. During the hot rolling process, the compression ratio is controlled at ≥6, the surface temperature of the initial rolling is controlled at 1100~1150℃, and the surface temperature of the hot rolling process and the final rolling is controlled at above 1000℃. The hot rolling is carried out in 5~13 passes, the deformation amount per pass is controlled at 8~15%, and the rolling speed is controlled at 1~1.2m / s.
2. The method for manufacturing a niobium-containing austenitic heat-resistant stainless steel round tube blank as described in claim 1, characterized in that, Between the continuous casting step and the billet heating step, there is also a billet surface inspection / grinding step, in which defects on the billet surface and within 0.5 mm below the surface are ground.
3. The method for manufacturing a niobium-containing austenitic heat-resistant stainless steel round tube blank as described in claim 1, characterized in that, Through LF furnace refining, the chemical composition of the molten steel is adjusted by mass percentage as follows: C 0.07~0.13%, Si≤0.30%, Mn≤1.00%, P≤0.035%, S≤0.010%, Cr 17.00~19.00%, Ni 8.50~10.50%, Mo 0.15~0.30%, Cu 2.50~3.50%, Nb 0.30~0.60%, N 0.05~0.15%, B 0.001~0.010%, Al 0.003~0.030%, [O]≤30ppm, with the remainder being Fe and unavoidable impurities.
4. The method for manufacturing a niobium-containing austenitic heat-resistant stainless steel round tube blank as described in any one of claims 1 to 3, characterized in that, The continuous casting billet obtained in the continuous casting step is a circular continuous casting billet with a diameter of Φ240~350mm or a square or rectangular continuous casting billet with a cross-sectional side length of (200~300mm)×(200~300mm).
5. The method for manufacturing a niobium-containing austenitic heat-resistant stainless steel round tube blank as described in claim 4, characterized in that, The proportion of the equiaxed crystal zone in the core of the continuously cast billet obtained by the continuous casting step is more than 20% of the cross-sectional area of the billet, and the proportion of the central porosity and shrinkage cavity defect area is less than 5% of the cross-sectional area of the billet.
6. The method for manufacturing a niobium-containing austenitic heat-resistant stainless steel round tube blank as described in claim 4, characterized in that, The round tube blank obtained in the hot-rolled round tube blank step is a round tube blank with a diameter of 85~110mm.
7. The method for manufacturing a niobium-containing austenitic heat-resistant stainless steel round tube blank as described in claim 6, characterized in that, The cross-sectional grain size of the round tube blank obtained by the hot-rolled round tube blank step is level 5 to 8, and the grain size difference is within 2 levels.
Citation Information
Patent Citations
Processing method of niobium-containing austenite heat-resistant stainless steel round tube blank
CN113399461A
High-purity smelting method for niobium-containing austenitic stainless steel
CN116287956A