Fiber reinforced copper-based self-lubricating composite material and preparation method thereof
By weaving a fiber framework in a cryogenic mold and performing bidirectional solidification, a fiber-reinforced copper-based self-lubricating composite material with fibers perpendicular to and oriented to the particle direction was prepared, which solved the problem of insufficient friction performance in the prior art and achieved low friction and low wear effect of the material.
Patent Information
- Application Number
- CN202410307141.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-18
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-03-18
AI Technical Summary
Existing technologies struggle to achieve the perpendicular and oriented arrangement of fibers and particles in fiber-reinforced copper-based self-lubricating composites, resulting in insufficient friction performance.
A fiber-reinforced copper-based self-lubricating composite material was prepared by using a cryogenic mold to weave a fiber framework and then performing bidirectional solidification, combined with vacuum drying, organic matter removal, and heat treatment. The fibers are perpendicular to the particle direction and oriented.
The material's friction coefficient is reduced, the wear rate is significantly reduced, and the fibers are uniformly distributed and oriented in the matrix, which improves the material's friction performance.
Smart Images

Figure CN118291890B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of metal matrix composite material preparation technology, and in particular to a fiber-reinforced copper-based self-lubricating composite material and its preparation method. Background Technology
[0002] Metal-based self-lubricating composites combine the excellent thermal and electrical conductivity, outstanding mechanical properties, and wear resistance of metals with the superior lubrication and friction-reducing properties of solid lubricants, thus possessing broad application potential in aerospace, automotive, and machinery industries. In particular, fiber-reinforced copper-based self-lubricating composites, due to their lower manufacturing cost, superior corrosion resistance, and ease of processing, coupled with the inherent good mechanical and tribological properties of the composite material itself, are frequently used in components such as spot welding electrodes, bearings, integrated circuit lead frames, and contact elements for electronic communication devices.
[0003] The lubricating phase particles used in self-lubricating composites exhibit typical 2D structural characteristics, resulting in good tribological properties when sliding parallel to the particle plane. Currently, the main methods for manufacturing fiber-reinforced copper-based self-lubricating composites include powder metallurgy, liquid metal hot extrusion, and template methods. Powder metallurgy is a commonly used method for preparing metal-based self-lubricating materials due to its advantages such as simple process, convenient operation, high material utilization, and high designability of material composition. However, its mechanical ball milling process cannot cause particle rearrangement in the matrix, leading to disorder of the lubricating phase particles in the matrix. Liquid metal hot extrusion requires high preparation temperatures and specialized equipment, and the resulting composite material only exhibits a certain degree of directional arrangement of lubricating particles. Template methods are a highly effective method for the directional assembly of particles of different scales (from nanoscale to microscale), and suitable template agents can be selected according to requirements to obtain the target structural material. For example, Wu et al. obtained copper-based composites with directional particle arrangement using the ice crystal template method, but the friction coefficient and friction rate parallel to the particle alignment direction need to be reduced. Summary of the Invention
[0004] The purpose of this invention is to provide a fiber-reinforced copper-based self-lubricating composite material with fibers and particles arranged perpendicularly and in a directional manner, and a method for preparing the same, so as to solve the problems existing in the prior art and to greatly improve the friction performance of the material perpendicular to the fiber arrangement direction or parallel to the particle orientation direction.
[0005] To achieve the above objectives, the present invention adopts the following technical solution: A method for preparing a fiber-reinforced copper-based self-lubricating composite material includes the following steps: Step 1: Weave the fiber bundles in a freezing mold along the direction perpendicular to the directional growth of the particles to obtain a freezing mold with a fiber frame. Step 2: Add the mixed slurry of the green material to a freeze mold with a fiber frame for bidirectional solidification. After freezing, vacuum dry to obtain the green material. Press the green material into shape, then remove organic matter, reduce the copper particles, and sinter to obtain a fiber-reinforced copper-based self-lubricating composite material with oriented particle arrangement.
[0006] Preferably, the fiber is either carbon fiber or glass fiber.
[0007] Preferably, the diameter of the fiber bundle is 0.2 mm to 0.4 mm.
[0008] Preferably, the fibers are first braided into bundles, and the diameter of the fibers is 5~6μm.
[0009] Preferably, the interval between adjacent fiber bundles is 2-4 mm.
[0010] Preferably, the preparation steps of the mixed slurry are as follows: a. Weigh out the reinforcing phase powder, copper or copper alloy powder, binder, dispersant and water according to the stoichiometric ratio; b. Divide the amount of deionized water in the formula into two portions, take one portion to dissolve the dispersant, and mechanically ball-mill the dispersant solution with the reinforcing phase powder, copper or copper alloy powder. c. Take another portion of deionized water to dissolve the binder. After the binder is completely dissolved, add it to the reaction system of step b and continue ball milling to obtain a mixed slurry.
[0011] Preferably, the reinforcing phase powder is a material with 2D structural characteristics; the particle size of the reinforcing phase powder ranges from 0.1 to 50.0 μm. The binder is one or more of polyvinyl alcohol, polyacrylic acid, polyurethane, epoxy resin, and gelatin; the binder accounts for 0.1-10.0 wt% of the total water mass in the raw materials. The sum of the volumes of the copper or copper alloy powder and the reinforcing phase powder is 5-40 vol of the slurry volume, and the total volume of all powders accounts for 1-30 vol of the overall slurry volume.
[0012] Preferably, the material with the 2D structural properties is any one of graphite, molybdenum disulfide, or tungsten disulfide.
[0013] Preferably, the ball-to-material ratio during ball milling in both steps b and c is 2-5:1; the ball milling speed in step b is 50-150 rpm, and the ball milling time is 2-4 h; the ball milling speed in step c is 80 rpm-200 rpm, and the ball milling time is ≥20 h. The bidirectional solidification temperature field described in step two is constructed by upper and lower freezing ends and a wedge mold, wherein the temperature of the upper end is 5~25℃, the temperature of the lower end is -60~-5℃, the freezing time of the mixed slurry is greater than or equal to 4h, and the vacuum drying time is ≥24h; The pressing pressure is 10-20 MPa, and the pressing is carried out along the direction perpendicular to the particle arrangement. The reduction treatment temperature is 300-450℃, and the time is 2-6 hours; The sintering process is carried out in a hot press furnace, an isostatic pressing furnace, or an electric discharge plasma furnace; the sintering temperature is 600-900℃, the time is 5-120 min, and the sintering pressure is 10-50 MPa.
[0014] The present invention also provides a fiber-reinforced copper-based self-lubricating composite material prepared by the above preparation method, wherein the fibers are perpendicular to the direction of the particles and are oriented.
[0015] The present invention discloses the following technical effects: This invention involves pouring a prepared slurry into a cryogenic mold where fibers have already been woven; then, the driving force generated by the water crystallization process causes the particles in the slurry to aggregate into layered ice crystals and forces the reinforcing phase particles to rearrange; followed by low-temperature vacuum drying to obtain a layered porous green material; then, the green material is cold-pressed and heat-treated to remove and reduce the organic matter and oxidized particles contained in the material; finally, it is hot-pressed at a higher temperature to obtain a fiber-reinforced copper-based self-lubricating material with oriented particles. The material prepared by this invention has fibers that are uniformly distributed and oriented within the matrix, resulting in a reduced coefficient of friction parallel to the particle alignment direction and a significantly reduced wear rate. Attached Figure Description
[0016] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.
[0017] Figure 1 This is a schematic diagram of a freezing mold with a fiber frame in this invention. Detailed Implementation
[0018] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0019] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0020] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.
[0021] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be apparent to those skilled in the art. This specification and embodiments are merely exemplary.
[0022] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.
[0023] Unless otherwise specified, the term "parts" in this invention refers to parts by weight.
[0024] In the embodiments of the present invention, the mass percentage of copper in the copper or copper alloy powder is greater than or equal to 50.0%.
[0025] The freezing mold used in this application consists of a copper base with good thermal conductivity and an organic square mold (acrylic) with high thermal insulation. A wedge-shaped mold is placed on top of the base. The area of the metal base matches the size of the square mold, ranging from 10×10mm² to 100×100mm². Figure 1 A schematic diagram of a freezing mold with a fiber frame; The material of the wedge mold is one of cured epoxy resin, polytetrafluoroethylene, or polymethylsiloxane. Example 1
[0026] (1) Weaving fiber framework Carbon fibers with a diameter of 5 μm are braided into carbon fiber bundles with a diameter of 0.2 mm. The carbon fiber bundles are then cut into multiple 40 mm segments and braided in a cryogenic mold along the direction perpendicular to the directional growth of the particles. The fiber bundles are arranged in parallel in the mold, with a spacing of 2 mm between adjacent fiber bundles, to obtain a cryogenic mold with a fiber frame.
[0027] (2) Preparation of a uniformly dispersed slurry Add 6.2g WS2 powder (average particle size 5.0μm), 39.8g Cu powder (purity greater than 99.0%, average particle size 10.0μm), 0.2g dispersant (polyvinylpyrrolidone) and 50.0g deionized water to a mixing tank and ball mill for 2 hours (ball milling speed 100rpm, ball-to-material ratio 2:1); Meanwhile, add 50.0g of deionized water and 2.5g of gelatin to a beaker and place it in a drying oven at 60℃ to dissolve. After it is completely dissolved, pour it into the above mixing tank for ball milling (ball milling speed: 100rpm, ball-to-material ratio: 2:1). After ball milling for 20 hours, a stable mixed slurry is obtained.
[0028] (3) Preparation of porous green materials The mixed slurry was poured into a cryogenic mold with a fiber frame containing a wedge mold (angle of 15°), and the cryogenic mold containing the mixed slurry was placed in a directional temperature field (the temperature at the bottom of the mold was set to -40°C and the temperature at the top of the mold was set to 5°C) for bidirectional solidification. After the slurry was frozen and solidified, the mold was placed in a low-temperature vacuum dryer and dried at -30°C for 24 hours to obtain a layered porous green body material.
[0029] (4) Pressing and molding of green body, removal of organic matter and reduction treatment of copper particles After drying, the layered porous material is cut into cuboids of 12×34×24mm3 and placed into a steel mold of the corresponding size for cold pressing (pressure of 10MPa). The cold pressing is carried out along the direction perpendicular to the particle arrangement. Then, the square green blank is placed in a tube atmosphere furnace for the removal of organic matter and reduction of copper particles under hydrogen atmosphere (heat treatment temperature of 350℃, holding time of 4h).
[0030] (5) Sintering The sample obtained through the above process was placed in a graphite mold of appropriate size and subjected to spark plasma sintering (sintering pressure of 40 MPa, sintering temperature of 700℃, and sintering time of 5 min). The sintering process was carried out in a hot press furnace. A composite material was prepared in which WS2 particles and fiber bundles were uniformly distributed and the fiber direction was perpendicular to the particle growth direction and oriented in the matrix. Example 2
[0031] (1) Carbon fibers with a diameter of 6μm are braided into carbon fiber bundles with a diameter of 0.4mm. Then, the carbon fiber bundles are cut into multiple 40mm segments and braided in a freezing mold along the direction perpendicular to the directional growth of the particles. The fiber bundles are arranged in parallel in the mold, and the spacing between adjacent fiber bundles is 3mm, thus obtaining a freezing mold with a fiber frame.
[0032] (2) Preparation of a uniformly dispersed slurry 5.1g MoS2 (average particle size 5.0μm), 37.5g Cu30Ni alloy powder (nickel content 30.0%, particle size 5-25μm), 0.2g dispersant (polyvinylpyrrolidone) and 50.0g deionized water were added sequentially to a mixing tank and ball-milled for 3 hours (ball milling speed: 150rpm, ball-to-material mass ratio: 3:1). Meanwhile, 1.0g of epoxy resin and 50.0g of deionized water were added to a 100ml beaker and placed in a drying oven at 60℃ to dissolve. After complete dissolution, the mixture was poured into the above mixing tank for ball milling (ball milling speed: 80rpm, ball-to-material mass ratio: 3:1). After ball milling for 22 hours, a stable mixed slurry with good rheological properties was obtained.
[0033] (3) Preparation of porous green materials The mixed slurry was poured into a freezing mold containing a wedge mold (angle of 5°), and the freezing mold containing the slurry was placed in a directional temperature field (the temperature at the bottom of the mold was set to -60°C and the temperature at the top was set to 25°C) for bidirectional solidification. After the slurry was frozen and solidified, the mold was placed in a low-temperature vacuum dryer and dried at -5°C for 24 hours to obtain a layered porous material.
[0034] (4) Pressing and molding of green body, removal of organic matter and reduction treatment of copper particles After drying, the layered porous material is cut into cuboids of 12×34×24mm3 and placed into a steel mold of the corresponding size for cold pressing (pressure of 15MPa). The cold pressing is carried out along the direction perpendicular to the particle arrangement. Then, the square green blank is placed in a tube atmosphere furnace for the removal of organic matter and reduction of copper particles under hydrogen atmosphere (heat treatment temperature of 450℃ and holding time of 2h).
[0035] (5) Sintering The samples obtained through the above process were placed in a graphite mold of appropriate size for spark plasma sintering (sintering pressure 10 MPa, sintering temperature 600℃, sintering time 120 min) in an isostatic pressing furnace. This resulted in the preparation of a Cu-MoS2 composite material with uniformly distributed MoS2 particles and fiber bundles, and the fiber direction perpendicular to the particle growth direction, oriented within the matrix.
[0036] This invention increases wear resistance by adding fibers arranged perpendicular to the grain growth direction. The thickness of the fiber bundles and the spacing between them can affect the wear resistance effect. This invention has obtained the optimal parameter values through long-term research.
[0037] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.
Claims
1. A method for producing a fiber-reinforced copper-based self-lubricating composite material, characterized by, Includes the following steps: Step 1: Weave the fiber bundles in a cryogenic mold along the direction perpendicular to the directional growth of the reinforcing phase particles to obtain a cryogenic mold with a fiber framework. Step 2: Add the mixed slurry of the green material to a freeze mold with a fiber frame for bidirectional solidification. After freezing, vacuum dry to obtain the green material. Press the green material into shape, then remove organic matter, reduce the copper particles, and sinter to obtain a fiber-reinforced copper-based self-lubricating composite material with oriented particle arrangement. The preparation steps of the mixed slurry are as follows: a. Weigh out the reinforcing phase powder, copper or copper alloy powder, binder, dispersant and water according to the stoichiometric ratio; b. Divide the amount of deionized water in the formula into two portions, take one portion to dissolve the dispersant, and mechanically ball-mill the dispersant solution with the reinforcing phase powder, copper or copper alloy powder. c. Take another portion of deionized water to dissolve the binder. After the binder is completely dissolved, add it to the reaction system of step b and continue ball milling to obtain a mixed slurry.
2. The method of producing a fiber-reinforced copper-based self-lubricating composite material according to claim 1, characterized by, The fiber can be either carbon fiber or glass fiber.
3. The method of producing a fiber-reinforced copper-based self-lubricating composite material according to claim 1, characterized by, The diameter of the fiber bundle is 0.2 mm to 0.4 mm.
4. The method of producing a fiber-reinforced copper-based self-lubricating composite material according to claim 1, characterized by, The fibers are first braided into bundles, with a diameter of 5~6μm.
5. The method for preparing the fiber-reinforced copper-based self-lubricating composite material according to claim 1, characterized in that, The spacing between adjacent fiber bundles is 2~4mm.
6. The method for preparing the fiber-reinforced copper-based self-lubricating composite material according to claim 1, characterized in that, The reinforcing phase powder is a material with 2D structural characteristics; the particle size of the reinforcing phase powder ranges from 0.1 to 50.0 μm. The binder is one or more of polyvinyl alcohol, polyacrylic acid, polyurethane, epoxy resin, and gelatin; the binder accounts for 0.1-10.0 wt% of the total water mass in the raw materials. The sum of the volumes of the copper or copper alloy powder and the reinforcing phase powder is 5-40 vol of the slurry volume, and the total volume of all powders accounts for 1-30 vol of the overall slurry volume.
7. The method for preparing the fiber-reinforced copper-based self-lubricating composite material according to claim 6, characterized in that, The material for the 2D structural properties is any one of graphite, molybdenum disulfide, or tungsten disulfide.
8. The method for preparing the fiber-reinforced copper-based self-lubricating composite material according to claim 6, characterized in that, In steps b and c, the ball-to-material ratio during ball milling is 2-5:1; in step b, the ball milling speed is 50-150 rpm and the ball milling time is 2-4 hours; in step c, the ball milling speed is 80-200 rpm and the ball milling time is ≥20 hours. The bidirectional solidification temperature field described in step two is constructed by upper and lower freezing ends and a wedge mold, wherein the temperature of the upper end is 5~25℃, the temperature of the lower end is -60~-5℃, the freezing time of the mixed slurry is greater than or equal to 4h, and the vacuum drying time is ≥24h; The pressing pressure is 10-20 MPa, and the pressing is carried out along the direction perpendicular to the arrangement of the reinforcing phase particles; The reduction treatment temperature is 300-450℃, and the time is 2-6 hours; The sintering process is carried out in a hot press furnace, an isostatic pressing furnace, or an electric discharge plasma furnace; the sintering temperature is 600-900℃, the time is 5-120 min, and the sintering pressure is 10-50 MPa.
9. A fiber-reinforced copper-based self-lubricating composite material prepared by the preparation method according to any one of claims 1-8, wherein the fibers are perpendicular to and oriented with respect to the direction of the reinforcing phase particles.
Citation Information
Patent Citations
Particle directional arrangement reinforced copper-based self-lubricating composite material and preparation method thereof
CN113774249A
Method for production of fiber-reinforced metal composite material
US4681151A