Method for producing an anti-coking coating, anti-coking coating and cracking device and use

By generating a three-layer anti-coking coating of silicon oxide, chromium oxide, and manganese chromium spinel on the surface of the alloy furnace tube, the high cost and low efficiency of coking in the prior art are solved, achieving efficient coking suppression and extended furnace tube life.

CN118291914BActive Publication Date: 2026-11-20CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310007596.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-04
Publication Date
2026-11-20
Estimated Expiration
2043-01-04

AI Technical Summary

Technical Problem

Existing anti-coking coatings are costly to prepare and have poor anti-coking performance, leading to frequent coking removal during ethylene production, which reduces production efficiency and shortens the life of cracking furnace tubes.

Method used

Using alloy furnace tubes with specific Si and Mn contents, a three-layer structure of silicon oxide, chromium oxide, and manganese chromium spinel is generated on the surface of the alloy furnace tube through a heat treatment process with low oxygen partial pressure and oxidizing gas, forming a dense and uniform anti-coking coating.

Benefits of technology

Significantly reduces coking, extends the life of pyrolysis furnace tubes, lowers production costs, and improves production efficiency, with a coking reduction rate of no less than 80%, and up to 90% in the preferred scheme.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present application relates to the field of cracking furnace, discloses a kind of preparation method of anti-coking coating and anti-coking coating and cracking device and application.The method comprises: using treatment gas to heat treatment alloy furnace tube, generate anti-coking coating;The elemental composition of the alloy furnace tube is that Cr content is 12-50wt%, Ni content is 20-50wt%, Si content 1.2-2.5wt%, Mn content 1.2-2.5wt%, C content is 0.2-0.6wt%, trace element 0.001-5wt%, the balance is Fe;Wherein, the surface roughness of the alloy furnace tube is 0.8-3 μm;The treatment gas contains oxidizing gas and low oxygen partial pressure gas.The preparation method is simple to operate, and by specific processing process, cooperate specific Si content and specific Mn content and specific roughness alloy furnace tube, the anti-coking coating prepared has excellent anti-coking performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of pyrolysis furnaces, and more specifically, to a method for preparing an anti-coking coating, as well as the anti-coking coating, pyrolysis apparatus, and its application. Background Technology

[0002] During ethylene production, surface coking and metal matrix carburization inevitably occur on the inner wall of the cracking furnace tubes, leading to two adverse consequences. Firstly, coking reduces the inner diameter of the furnace tubes, increases pressure drop, decreases the unit's throughput, and increases the tube wall thermal resistance, lowering the heat transfer coefficient and increasing energy consumption. Therefore, the cracking furnace typically requires shutdown for decoking every 30-60 days. This frequent decoking significantly reduces production efficiency and increases production costs. Secondly, the carbon deposited on the furnace tube surface diffuses into the metal matrix, forming carbides, increasing material brittleness, and potentially causing metal powdering. This material damage caused by carburization interacts with the thermal cycle during decoking, greatly shortening the lifespan of the cracking furnace tubes. Therefore, furnace tube coking is a pressing problem that needs to be solved in ethylene production.

[0003] Based on the coking mechanism, the main methods used domestically and internationally to inhibit coking currently include adding coking inhibitors, surface pretreatment technology, new furnace tubes, and enhanced heat transfer technology. Whether it's adding coking inhibitors, surface pretreatment, or enhanced heat transfer, these methods primarily target furnace tubes made of commonly used HK-40, HP-40, HP-45, and 35Cr45Ni steel. Improving the furnace tube material can not only inhibit surface catalytic coking but also effectively improve the furnace tube's heat transfer efficiency, significantly reducing coking. The most typical example is the ceramic pyrolysis furnace tubes developed by S&W and Linde, which can avoid coking problems from the coking mechanism perspective. Incoloy's MA956 alloy (Fe-20Cr-45Al-0.5Ti-0.5Y2O3) not only has high creep strength but also effectively inhibits coking and carburization. On a laboratory scale, this new furnace tube material reduces coking rate by 50% and almost eliminates carburization compared to ordinary 25Cr35Ni alloy. The Swedish company Sandvik has developed a modified radiant tube, APMT, made from Fe-Cr-Al alloy through a rapid solidification process. This improved material exhibits superior resistance to carburization, reducing coke formation, extending operating cycles, and increasing ethylene yield. The iron-based thermally resistant oxidation diffusion-enhanced (ODS) alloy, jointly developed by JGC and Special Metals, possesses high creep strength and corrosion resistance, extending the operating cycle of pyrolysis furnaces and increasing production capacity. Oak Ridgel National Laboratory in the United States has developed a new pyrolysis furnace tube material. This material has a 3.2mm thick aluminum compound coating on its surface. During the tube manufacturing process, the aluminum compound is incorporated into the tube through co-extrusion and co-casting, resulting in an order of magnitude improvement in coking suppression and carburization prevention compared to ordinary Cr-Ni stainless steel furnace tubes.

[0004] However, the above methods have high production costs, and ceramic materials are brittle with a significantly different coefficient of thermal expansion compared to metals, making them prone to cracking when welded to metals in the equipment. APMT technology, ODS alloys, and new aluminum-doped furnace tube materials primarily work by oxidizing the aluminum in the alloy to form an alumina layer on the metal surface, thereby improving the metal's oxidation and coking resistance. However, alumina generally has limited anti-coking properties and a limited ability to reduce cracking and coking. Summary of the Invention

[0005] The purpose of this invention is to overcome the problems of high preparation cost and poor anti-coking performance of existing anti-coking coatings, and to provide a method for preparing an anti-coking coating, as well as the anti-coking coating, pyrolysis device and application. The preparation method is simple to operate, and through specific processing technology, combined with alloy furnace tubes with specific Si content, specific Mn content and specific roughness, the prepared anti-coking coating has excellent anti-coking performance.

[0006] To achieve the above objectives, the first aspect of the present invention provides a method for preparing an anti-coking coating, characterized in that the method includes: heat-treating an alloy furnace tube with a processing gas to generate an anti-coking coating;

[0007] The alloy furnace tube has the following elemental composition: Cr content 12-50wt%, Ni content 20-50wt%, Si content 1.2-2.5wt%, Mn content 1.2-2.5wt%, C content 0.2-0.6wt%, trace elements 0.001-5wt%, and the balance being Fe.

[0008] The surface roughness of the alloy furnace tube is 0.8-3 μm;

[0009] The processing gas contains oxidizing gases and gases with low oxygen partial pressure.

[0010] The second aspect of the present invention provides an anti-coking coating prepared by the method of the first aspect, characterized in that the anti-coking coating has a three-layer structure, which consists of a silicon oxide layer, a chromium oxide layer and a manganese chromium spinel layer in sequence along the direction from the inner wall of the alloy furnace tube to the surface.

[0011] A third aspect of the present invention provides a pyrolysis apparatus, characterized in that the inner wall of the pyrolysis apparatus comprises the anti-coking coating described in the second aspect.

[0012] The fourth aspect of this invention provides a method for preparing the anti-coking coating described in the first aspect, the application of the anti-coking coating described in the second aspect and the pyrolysis device described in the third aspect in a hydrocarbon thermal pyrolysis process.

[0013] Through the above technical solutions, the method for preparing the anti-coking coating, the anti-coking coating and the pyrolysis device and application provided by the present invention achieve the following beneficial effects: by using a processing gas containing oxidizing gas and low oxygen partial pressure gas to heat treat an alloy furnace tube containing specific Si content, specific Mn content and specific roughness, the prepared anti-coking coating can be made to have a suitable thickness and excellent anti-coking performance. Detailed Implementation

[0014] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0015] The first aspect of the present invention provides a method for preparing an anti-coking coating, characterized in that the method includes: heat-treating an alloy furnace tube with a processing gas to generate an anti-coking coating;

[0016] The alloy furnace tube has the following elemental composition: Cr content 12-50wt%, Ni content 20-50wt%, Si content 1.2-2.5wt%, Mn content 1.2-2.5wt%, C content 0.2-0.6wt%, trace elements 0.001-5wt%, and the balance being Fe.

[0017] The surface roughness of the alloy furnace tube is 0.8-3 μm;

[0018] The processing gas contains oxidizing gases and gases with low oxygen partial pressure.

[0019] In this invention, the processing gas contains oxidizing gas and low oxygen partial pressure gas, and is heat-treated with alloy furnace tubes of specific Si and Mn contents. This process generates a uniform and dense anti-coking and anti-carburizing coating on the inner surface of the alloy furnace tube, which has excellent anti-coking properties.

[0020] In this invention, the inventors discovered that when the Si content in the alloy furnace tube is too low, a discontinuous silicon dioxide layer is formed, leading to the rapid formation of a large amount of Cr and Mn oxides during the oxidizing atmosphere treatment, resulting in the peeling off of the oxide film. When the Si content is too high, a dense and continuous silicon dioxide layer is formed, resulting in only a small amount of Cr and Mn migrating to the substrate surface during the oxidizing atmosphere treatment, causing only a portion of the alloy surface to be able to form a manganese chromium spinel film.

[0021] Similarly, in alloy furnace tubes, excessively low Mn content leads to a low Mn content on the surface of the anti-coking coating after treatment, hindering the formation of a good manganese-chromium spinel film. Excessively high Mn content negatively impacts the alloy's mechanical properties, and further increases in the matrix do not significantly increase the surface Mn content after treatment. Therefore, achieving the optimal anti-coking coating requires Si and Mn contents within the aforementioned ranges.

[0022] According to the present invention, the heat treatment conditions include: firstly, performing a first heat treatment on the alloy furnace tube using a low oxygen partial pressure gas, and then performing a second heat treatment on the alloy furnace tube using an oxidizing gas.

[0023] In this invention, the inventors discovered that under a low oxygen partial pressure atmosphere, Si in the alloy furnace tube most readily reacts with oxygen to form a silicon oxide layer, which forms a protective film. This film prevents Fe and Ni from migrating to the alloy surface and reacting with oxidizing gases to form iron oxide and nickel oxide during the second heat treatment. During the second heat treatment, Mn and Cr in the matrix gradually diffuse through the silicon oxide layer to the alloy surface and oxidize to form chromium oxide and manganese oxide. Due to the rapid migration rate of Mn in chromium oxide, Mn forms manganese oxide on the outermost layer. At high temperatures, manganese oxide and chromium oxide further form manganese-chromium spinel oxide, which has better thermodynamic stability.

[0024] Therefore, the alloy furnace tube is first subjected to a low-oxygen partial pressure gas for heat treatment. Since Si combines more readily with O, a silicon oxide layer will first form on the inner wall surface of the alloy furnace tube. The thickness of this silicon oxide layer will further affect the amount of Cr and Mn elements migrating to the surface of the alloy furnace tube, so controlling the content of Si and Mn is crucial. A second heat treatment of the alloy furnace tube with an oxidizing gas can prepare an anti-coking coating with excellent anti-coking properties while improving safety and saving costs.

[0025] According to the present invention, the conditions for the first heat treatment include: a temperature of 600-1200°C and a time of 0.5-2 hours.

[0026] Furthermore, the conditions for the first heat treatment include: a temperature of 950-1000℃ and a time of 1-2 hours.

[0027] According to the present invention, the conditions for the second heat treatment include: a temperature of 600-1200°C and a time of 5-50 hours.

[0028] Furthermore, the conditions for the second heat treatment include: a temperature of 950-1000℃ and a time of 10-30h.

[0029] According to the present invention, the oxidizing gas comprises oxygen and a protective gas.

[0030] According to the present invention, the oxidizing gas contains 0.1-50 vol% oxygen and 50-99.9 vol% protective gas.

[0031] In this invention, the content of oxygen and protective gas meets the above-mentioned range, which can fully oxidize Cr and Mn elements, and further prepare an anti-coking coating with suitable thickness and excellent anti-coking performance.

[0032] Furthermore, the oxidizing gas contains 10-30 vol% oxygen and 70-90 vol% protective gas.

[0033] In this invention, the protective gas is not particularly limited and can be nitrogen or an inert gas commonly used in the art, such as Ar.

[0034] In this invention, from the perspective of cost saving, the oxidizing gas is more preferably air.

[0035] In this invention, the inventors discovered that the conditions of the second heat treatment have a significant impact on the performance of the obtained anti-coking coating. For example, when the Si content in the alloy furnace tube is high, appropriately increasing the temperature of the second treatment and increasing the oxygen content in the oxidizing gas can still produce an anti-coking coating with high anti-coking performance.

[0036] Preferably, the conditions for the second heat treatment include: a temperature of 960-1000℃ and a time of 10-30h.

[0037] According to the present invention, the low-oxygen partial pressure gas is selected from at least one of alkanes, hydrogen, CO and water vapor.

[0038] Furthermore, the low-oxygen partial pressure gas is selected from hydrogen and water vapor.

[0039] Furthermore, the volume ratio of the hydrogen to the water vapor is 33.3-99.8:1.

[0040] According to the present invention, the partial pressure of oxygen in the low-oxygen partial pressure gas is ≤10. -12 atm.

[0041] In this invention, the partial pressure of oxygen in the low-oxygen partial pressure gas meets the above-mentioned range, which can generate a dense and uniform anti-coking coating.

[0042] Furthermore, the partial pressure of oxygen in the low-oxygen partial pressure gas is 10. -34 -10 -13 atm.

[0043] According to the present invention, the elemental composition of the alloy furnace tube is 23-37 wt% Cr, 33-48 wt% Ni, 1.25-1.75 wt% Si, 1.25-1.75 wt% Mn, 0.3-0.5 wt% C, 1-3 wt% trace elements, and the balance being Fe.

[0044] Furthermore, the trace element is selected from at least one of Al, Nb, Ti, W, Mo and rare earth elements.

[0045] According to the present invention, the surface roughness of the alloy furnace tube is 0.8-2.5 μm.

[0046] The second aspect of the present invention provides an anti-coking coating prepared by the method of the first aspect, characterized in that the anti-coking coating has a three-layer structure, which consists of a silicon oxide layer, a chromium oxide layer and a manganese chromium spinel layer in sequence along the direction from the inner wall of the alloy furnace tube to the surface.

[0047] In this invention, the thickness ratio of the silicon oxide layer, the chromium oxide layer, and the manganese chromium spinel layer is 0.14-7:0.14-7:1.

[0048] In this invention, the inventors discovered that the thickness of the silicon oxide layer is a key factor affecting the thickness and integrity of the manganese chromium spinel layer. Through research, it was found that when the thickness ratio of the silicon oxide layer, the chromium oxide layer, and the manganese chromium spinel layer meets the above-mentioned range, a uniform and dense manganese chromium spinel oxide film can be obtained, which makes the anti-coking coating have excellent anti-coking performance.

[0049] Furthermore, the thickness ratio of the silicon oxide layer, the chromium oxide layer, and the manganese chromium spinel layer is 0.3-3:0.3-3:1.

[0050] In this invention, the mass ratio of Cr to Mn in the manganese chromium spinel layer is 0.5-3.1:1, preferably 1.5-2.55:1; the total content of Fe and Ni is ≤20wt%, preferably ≤15wt%.

[0051] According to a particularly preferred embodiment of the present invention, the method comprises: using a hydrogen:water vapor mixture with a volume ratio of 33.3-99.8:1 at 950-1000°C and an oxygen partial pressure of 10. -34 -10 -13 The alloy furnace tube is subjected to a first heat treatment at ATM for 1-2 hours, and then subjected to a second heat treatment at 950-1000℃ for 10-30 hours in an air atmosphere (oxygen content of 10-30 vol%) to generate an anti-coking coating.

[0052] The elemental composition of the alloy furnace tube is as follows (wt%): Al: 0.5-1.5, Si: 1.25-1.75, Mn: 1.25-1.75, Cr: 26-36, Ni: 34-46, C: 0.3-0.5, Nb: 0.8-1.5, with the balance being Fe;

[0053] The surface roughness of the alloy furnace tube is 0.8-2.5 μm;

[0054] The anti-coking coating has a three-layer structure, consisting of a silicon oxide layer, a chromium oxide layer, and a manganese-chromium spinel layer, arranged sequentially from the inner wall of the alloy furnace tube to its surface. The thickness ratio of the silicon oxide layer, the chromium oxide layer, and the manganese-chromium spinel layer is 0.14-7:0.14-7:1.

[0055] The Cr / Mn mass ratio in the manganese chromium spinel layer is 1.5-2.55:1, and the total content of Fe and Ni is 10-15 wt%.

[0056] A third aspect of the present invention provides a pyrolysis apparatus, characterized in that the inner wall of the pyrolysis apparatus comprises the anti-coking coating described in the second aspect.

[0057] In this invention, the anti-coking coating has a coverage of ≥80wt% on the inner wall of the pyrolysis device, preferably ≥85wt%.

[0058] The fourth aspect of this invention provides a method for preparing the anti-coking coating described in the first aspect, the application of the anti-coking coating described in the second aspect and the pyrolysis device described in the third aspect in a hydrocarbon thermal pyrolysis process.

[0059] In this invention, the coking reduction rate of the alloy furnace tube containing the anti-coking coating provided by this invention is not less than 80%, and preferably 85-90%, compared with the alloy furnace tube without the anti-coking coating.

[0060] The present invention will be described in detail below through embodiments. In the following embodiments, alloy materials with the same material and elemental composition as the alloy furnace tubes in the embodiments and comparative examples were used, and anti-coking coatings were generated in situ using the methods of the embodiments and comparative examples for testing.

[0061] The elemental composition and coverage of the alloy material were determined using X-ray energy dispersive spectroscopy (EDS).

[0062] The surface roughness of alloy materials is measured using a roughness measuring instrument;

[0063] The thickness of the anti-coking coating on the alloy material was measured by scanning electron microscopy (SEM).

[0064] The amount of coking in the alloy furnace tube was calculated by measuring the concentrations of CO and CO2 in the coking gas online using an infrared instrument and by measuring the volume of the coking gas online using a wet gas flow meter.

[0065] Example 1

[0066] Using a hydrogen:water vapor ratio of 98:1 at 950℃, with an oxygen partial pressure of 5 × 10⁻⁶... -20 The alloy furnace tube with a roughness of 2.5 μm was subjected to a first heat treatment for 1 h at ATM, and then subjected to a second heat treatment at 950 °C for 20 h in an air atmosphere (oxygen content of 21 vol%). The elemental composition of the alloy furnace tube is (wt%): Al: 1, Si: 1.5, Mn: 2, Cr: 33.2, Ni: 41.3, C: 0.4, Nb: 0.98, with the balance being Fe.

[0067] A three-layer anti-coking coating of silicon oxide / chromium oxide / manganese chromium spinel is formed along the direction from the inner wall to the surface of the alloy furnace tube. The thickness ratio of the silicon oxide layer, the chromium oxide layer, and the manganese chromium spinel layer is 1.1:1.4:1.

[0068] The manganese chromium spinel layer contains 45.95 wt% Cr, 19.17 wt% Mn, with a Cr / Mn mass ratio of 2.4:1 and a total Fe and Ni content of 10.8 wt%.

[0069] The anti-coking coating has a coverage of 89.2 wt% on the inner wall of the pyrolysis unit.

[0070] Example 2

[0071] The method is consistent with that of Example 1, except that the elemental composition of the alloy furnace tube is (wt%): Al: 0.8, Si: 2, Mn: 1.5, Cr: 32.4, Ni: 42.5, C: 0.5, Nb: 0.88, with the balance being Fe. The conditions for the second heat treatment include: performing the second heat treatment at 970°C for 30 hours in an oxidizing atmosphere (oxygen content of 30 vol%).

[0072] A three-layer anti-coking coating of silicon oxide / chromium oxide / manganese chromium spinel is formed along the direction from the inner wall to the surface of the alloy furnace tube. The thickness ratio of the silicon oxide layer, the chromium oxide layer, and the manganese chromium spinel layer is 1:1.3:1.

[0073] The manganese chromium spinel layer contains 47.29 wt% Cr, 18.63 wt% Mn, with a Cr / Mn mass ratio of 2.54:1 and a total Fe and Ni content of 10.3 wt%.

[0074] The anti-coking coating has a coverage of 89.7 wt% on the inner wall of the pyrolysis unit.

[0075] Example 3

[0076] The method is the same as in Example 1, except that the elemental composition of the alloy furnace tube is (wt%): Al: 1.2, Si: 1.5, Mn: 1.2, Cr: 32.5, Ni: 43.6, C: 0.4, Nb: 0.93, with the balance being Fe.

[0077] A three-layered anti-coking coating of silicon oxide / chromium oxide / manganese chromium spinel is formed along the inner wall of the alloy furnace tube to its surface. The thickness ratio of the silicon oxide layer, the chromium oxide layer, and the manganese chromium spinel layer is 1.2:1.6:1.

[0078] The manganese chromium spinel layer contains 41.89 wt% Cr, 17.07 wt% Mn, with a Cr / Mn mass ratio of 2.45:1 and a total Fe and Ni content of 16.36 wt%.

[0079] The anti-coking coating has a coverage of 83.64 wt% on the inner wall of the pyrolysis unit.

[0080] Example 4

[0081] The method is the same as in Example 1, except that the elemental composition of the alloy furnace tube is (wt%): Al: 0.9, Si: 1.2, Mn: 1.7, Cr: 32.6, Ni: 44.7, C: 0.5, Nb: 0.9, with the balance being Fe.

[0082] A three-layer anti-coking coating of silicon oxide / chromium oxide / manganese chromium spinel is formed along the direction from the inner wall to the surface of the alloy furnace tube. The thickness ratio of the silicon oxide layer, the chromium oxide layer, and the manganese chromium spinel layer is 1.1:1.5:1.

[0083] The manganese chromium spinel layer contains 49.08 wt% Cr, 15.89 wt% Mn, with a Cr / Mn mass ratio of 3.09:1 and a total Fe and Ni content of 12.98 wt%.

[0084] The anti-coking coating has a coverage of 87.02 wt% on the inner wall of the pyrolysis unit.

[0085] Example 5

[0086] The method is the same as in Example 1, except that the conditions for the first heat treatment are: 900°C and an oxygen partial pressure of 5 × 10⁻⁶. - 20 The alloy furnace tube with a roughness of 2.5 μm was subjected to a first heat treatment for 0.5 h at ATM.

[0087] A three-layer anti-coking coating of silicon oxide / chromium oxide / manganese chromium spinel is formed along the inner wall of the alloy furnace tube to its surface. The thickness ratio of the silicon oxide layer, the chromium oxide layer, and the manganese chromium spinel layer is 0.7:1.3:1.

[0088] The manganese chromium spinel layer contains 40.21 wt% Cr, 16 wt% Mn, with a Cr / Mn mass ratio of 2.51:1 and a total Fe and Ni content of 16 wt%.

[0089] The anti-coking coating has a coverage of 84 wt% on the inner wall of the pyrolysis unit.

[0090] Example 6

[0091] The method is the same as in Example 1, except that the roughness of the alloy furnace tube is 3 μm.

[0092] A three-layered anti-coking coating of silicon oxide / chromium oxide / manganese chromium spinel is formed along the inner wall of the alloy furnace tube to its surface. The thickness ratio of the silicon oxide layer, the chromium oxide layer, and the manganese chromium spinel layer is 0.4:1.4:1.

[0093] The manganese chromium spinel layer contains 45 wt% Cr, 19 wt% Mn, with a Cr / Mn mass ratio of 2.36:1 and a total Fe and Ni content of 13 wt%.

[0094] The anti-coking coating has a coverage of 87 wt% on the inner wall of the pyrolysis unit.

[0095] Comparative Example 1

[0096] The method is the same as in Example 1, except that the elemental composition of the alloy furnace tube is (wt%): Al: 0.7, Si: 1.5, Mn: 1.1, Cr: 33.7, Ni: 41.2, C: 0.5, Nb: 0.85, with the balance being Fe.

[0097] A three-layered anti-coking coating of silicon oxide / chromium oxide / manganese chromium spinel is formed along the inner wall of the alloy furnace tube to its surface. The thickness ratio of the silicon oxide layer, the chromium oxide layer, and the manganese chromium spinel layer is 2.1:2.4:1.

[0098] The manganese chromium spinel layer contains 45.81 wt% Cr, 11.3 wt% Mn, with a Cr / Mn mass ratio of 4.06:1 and a total Fe and Ni content of 26.55 wt%.

[0099] The anti-coking coating has a coverage of 73.45 wt% on the inner wall of the pyrolysis unit.

[0100] Comparative Example 2

[0101] The method is the same as in Example 1, except that the elemental composition of the alloy furnace tube is (wt%): Al: 0.9, Si: 0.8, Mn: 1.8, Cr: 32.8, Ni: 43.7, C: 0.5, Nb: 0.92, with the balance being Fe.

[0102] A three-layered anti-coking coating of silicon oxide / chromium oxide / manganese chromium spinel is formed along the inner wall of the alloy furnace tube to its surface. The thickness ratio of the silicon oxide layer, the chromium oxide layer, and the manganese chromium spinel layer is 0.1:1.5:1.

[0103] The manganese chromium spinel layer contains 49.81 wt% Cr, 19.37 wt% Mn, with a Cr / Mn mass ratio of 2.57:1 and a total Fe and Ni content of 27.21 wt%.

[0104] The anti-coking coating has a coverage of 72.79 wt% on the inner wall of the pyrolysis unit.

[0105] Comparative Example 3

[0106] The method is the same as in Example 1, except that the elemental composition of the alloy furnace tube is (wt%): Al: 1.1, Si: 2.7, Mn: 1.2, Cr: 31.6, Ni: 43.9, C: 0.5, Nb: 0.94, with the balance being Fe.

[0107] A three-layered anti-coking coating of silicon oxide / chromium oxide / manganese chromium spinel is formed along the inner wall of the alloy furnace tube to its surface. The thickness ratio of the silicon oxide layer, the chromium oxide layer, and the manganese chromium spinel layer is 4:1.5:1.

[0108] The manganese chromium spinel layer contains 40.93 wt% Cr, 12.31 wt% Mn, with a Cr / Mn mass ratio of 3.32:1 and a total Fe and Ni content of 21.75 wt%.

[0109] The anti-coking coating has a coverage of 78.25 wt% on the inner wall of the pyrolysis unit.

[0110] Comparative Example 4

[0111] The method is the same as in Example 1, except that the roughness of the alloy furnace tube is 0.5 μm.

[0112] A three-layered anti-coking coating of silicon oxide / chromium oxide / manganese chromium spinel is formed along the inner wall of the alloy furnace tube to its surface. The thickness ratio of the silicon oxide layer, the chromium oxide layer, and the manganese chromium spinel layer is 1.8:1.3:1.

[0113] The manganese chromium spinel layer contains 41.89 wt% Cr, 17.07 wt% Mn, with a Cr / Mn mass ratio of 2.45:1 and a total Fe and Ni content of 23.2 wt%.

[0114] The anti-coking coating has a coverage of 76.8 wt% on the inner wall of the pyrolysis unit.

[0115] Test case

[0116] The furnace tubes with anti-coking coatings prepared in the examples and comparative examples were subjected to hydrocarbon steam cracking reactions, with naphtha as the cracking feedstock. At the same time, a blank furnace tube without anti-coking coating was used to conduct naphtha cracking experiments as a control.

[0117] Specifically, the naphtha feed rate is 100 g / h, the water feed rate is 50 g / h, the preheating temperature is 600℃, the pyrolysis temperature is 850℃, and the residence time is approximately 0.5 s.

[0118] After the pyrolysis experiment, the furnace tube temperature was controlled at 810-840℃, and coking was carried out using a mixture of N2 and O2 gas. The total amount of coking was calculated. The amount of coking in the blank furnace tube without the anti-coking coating was M0, and the amount of coking in the alloy furnace tube with the anti-coking coating provided by this invention was M1. The coking reduction rate was calculated using the formula: coking reduction rate = (M1-M0) / M0×100%.

[0119] The coking reduction rate of the embodiments and comparative examples of the present invention compared with the blank example is shown in Table 1.

[0120] Table 1

[0121] Coking reduction rate / % Example 1 90 Example 2 88 Example 3 87 Example 4 83 Example 5 85 Example 6 79 Comparative Example 1 60 Comparative Example 2 55 Comparative Example 3 77 Comparative Example 4 75

[0122] As can be seen from the results of Examples 1-6, Comparative Examples 1-4 and Table 1, Examples 1-6 of the present invention have good effects, and the coking reduction rate is not less than 79% compared with the blank example.

[0123] Furthermore, in Embodiment 1, which satisfies the preferred technical solution of the present invention, due to the suitable Si and Mn content, the generated anti-coking coating has suitable thicknesses and high coverage of the silicon oxide layer, chromium oxide layer, and manganese chromium spinel layer, resulting in higher anti-coking performance and a coking reduction rate of 90%. In Embodiment 2, the alloy furnace tube has a high Si content, but even under high processing temperature and high oxygen content conditions, a uniform anti-coking coating can still be obtained, with the manganese chromium spinel coverage reaching 89.7 wt% and a coking reduction rate of 88%.

[0124] In Comparative Examples 1-3, since the contents of Mn and Si do not meet the range defined by the present invention, the thickness ratio between silicon oxide / chromium oxide / manganese chromium spinel in the prepared anti-coking coating does not meet the requirements, and thus cannot have good anti-coking performance.

[0125] In Comparative Example 4, due to the low roughness of the alloy furnace tube, it is not easy to form a manganese-chromium spinel film. The total Fe and Ni content on the inner surface of the pyrolysis furnace tube is too high, and it cannot be effectively used to suppress coking in the furnace tube pyrolysis.

[0126] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A method for preparing an anti-coking coating, characterized in that, The method includes: heat-treating the alloy furnace tube with a processing gas to generate an anti-coking coating; The alloy furnace tube has the following elemental composition: Cr content 12-50wt%, Ni content 20-50wt%, Si content 1.5-2.5wt%, Mn content 1.2-2.5wt%, C content 0.2-0.6wt%, trace elements 0.001-5wt%, and the balance being Fe. The surface roughness of the alloy furnace tube is 0.8-3 μm; The processing gas contains oxidizing gases and gases with low oxygen partial pressure; The heat treatment conditions include: first, using a low oxygen partial pressure gas to perform a first heat treatment on the alloy furnace tube, and then using an oxidizing gas to perform a second heat treatment on the alloy furnace tube. The oxidizing gas includes oxygen and a protective gas; The oxidizing gas contains 0.1-50 vol% oxygen and 50-99.9 vol% protective gas. The partial pressure of oxygen in the low-oxygen partial pressure gas is ≤10. -12 atm.

2. The method according to claim 1, wherein, The conditions for the first heat treatment include: temperature 600-1200℃, time 0.5-2h.

3. The method according to claim 1, wherein, The conditions for the second heat treatment include: temperature 600-1200℃, time 5-50h.

4. The method according to any one of claims 1-3, wherein, The low-oxygen partial pressure gas is selected from at least one of alkanes, hydrogen, CO, and water vapor.

5. The method according to any one of claims 1-3, wherein, The low-oxygen partial pressure gas is hydrogen and water vapor.

6. The method according to claim 5, wherein, The volume ratio of hydrogen to water vapor is 33.3-99.8:

1.

7. The method according to any one of claims 1-3, wherein, The partial pressure of oxygen in the low-oxygen partial pressure gas is 10. -34 -10 -13 atm.

8. The method according to any one of claims 1-3, wherein, The trace elements are selected from at least one of Al, Nb, Ti, W, Mo and rare earth elements.

9. The method according to any one of claims 1-3, wherein, The surface roughness of the alloy furnace tube is 0.8-2.5 μm.

10. The anti-coking coating prepared by the method according to any one of claims 1-9, characterized in that, The anti-coking coating has a three-layer structure, consisting of a silicon oxide layer, a chromium oxide layer, and a manganese chromium spinel layer, arranged sequentially along the inner wall of the alloy furnace tube to the surface.

11. The anti-coking coating according to claim 10, wherein, The thickness ratio of the silicon oxide layer, the chromium oxide layer, and the manganese chromium spinel layer is 0.14-7:0.14-7:

1.

12. The anti-coking coating according to claim 10, wherein, In the manganese chromium spinel layer, the mass ratio of Cr to Mn is 0.5-3.1:1; the total content of Fe and Ni is ≤20wt%.

13. The anti-coking coating according to claim 10, wherein, In the manganese chromium spinel layer, the mass ratio of Cr to Mn is 1.5-2.55:1; the total content of Fe and Ni is ≤15wt%.

14. A pyrolysis apparatus, characterized in that, The inner wall of the pyrolysis device comprises an anti-coking coating as described in any one of claims 10-13.

15. The pyrolysis apparatus according to claim 14, wherein, The anti-coking coating has a coverage of ≥84wt% on the inner wall of the pyrolysis unit.

16. The pyrolysis apparatus according to claim 14, wherein, The anti-coking coating has a coverage of ≥85wt% on the inner wall of the pyrolysis unit.

17. The application of the anti-coking coating preparation method according to any one of claims 1-9, the anti-coking coating according to any one of claims 10-13, and the pyrolysis device according to any one of claims 14-16 in hydrocarbon thermal cracking processes.

Citation Information

Patent Citations

  • Method for treating inner surface of hydrocarbon cracking furnace tube

    CN112725009A

  • Surface on a stainless steel matrix

    US20050257857A1