Smart Images

Figure CN118292061B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chip packaging, and in particular to a copper electroplating solution for chip packaging and a preparation method thereof. Background Art
[0002] Integrated circuits (ICs) were developed in the 1960s. As the size of transistors continued to shrink, they evolved from small-scale integrated circuits (SSI), medium-scale integrated circuits (MSI), large-scale integrated circuits (LSI), to ultra-large-scale integrated circuits (ULSI). Whether it is a single transistor or an integrated circuit, it must be packaged to function. Packaging is the basis of system integration.
[0003] Electroplating copper is an important technology for chip packaging and is widely used in wiring (RDL), through silicon via technology (TSV) and bump filling. Additives are an important component of the electroplating solution and play an irreplaceable role in the electroplating process. Additives can effectively improve the current distribution during the electroplating process, improve the throwing power of the plating solution, and affect the transportation and electrocrystallization process of copper ions from the solution to the reaction interface, thereby changing the electrochemical deposition rate of the micro-concave and micro-convex parts of the board surface.
[0004] Electroplating copper additives generally include accelerators, inhibitors and levelers. Commonly used accelerators are mainly sodium polydisulfide propane sulfonate (SPS), sodium 3-mercapto-1-propane sulfonate (MPS), and sodium N,N-dimethyl-dithiocarbonyl propane sulfonate (DPS); inhibitors are polyethylene glycol (PEG), polypropylene glycol (PPG) and PEG-PPG copolymers; levelers are mainly dye levelers, such as Janus Green B (JGB), diazinon black (DB), etc., and organic amine levelers, such as benzotriazole (BAT), dodecyltrimethylammonium chloride (DTAC), polyethyleneimine alkyl salt (PN), triethylbenzylammonium chloride (TEBA), etc. The existing additive formula uses inhibitors and levelers in combination, such as the synergistic effect between the leveler JGB and the inhibitor PEG. The inhibitor is mainly a macromolecular polymer. Through a dense polymer film formed on the copper / electrolyte interface, during the electroplating process, this dense polymer film will not be incorporated into the deposited copper layer in large quantities, but will continue an adsorption-desorption process (desorbed from the old copper layer and adsorbed on the new copper layer), thereby continuously adsorbing on the surface of the newly deposited copper layer to act as a diffusion barrier to limit the diffusion of copper ions to the copper surface, thereby greatly reducing the copper deposition rate. The leveling agent is mainly a positively charged small molecule organic substance, which is adsorbed on the raised area with higher cathode current density to inhibit copper deposition and achieve the effect of leveling.
[0005] For better stability and reliability, electroplated copper filling requires no gaps or voids. However, when using DC electroplating to fill holes, the current density and convection intensity at the hole mouth are much higher than those inside the hole. The uneven current density leads to uneven plating, and the copper deposition rate at the hole mouth is much higher than that inside the hole, which will cause a sealing phenomenon, thus affecting product quality. Levelers usually carry a positive charge and can be adsorbed in areas of high electron density to inhibit copper deposition, which is essential for achieving super filling or bottom-up deposition. The levelers that have been developed are mainly organic dye levelers. Although this type of leveler can meet the filling effect under its specific conditions, the current levelers have the following problems: First, they must be used in combination with inhibitors, and other organic additives need to be added to the solution, making the solution composition complex. The stability of the organic additives affects the performance of the electroplating solution; second, the existing dye additives are toxic and pollute the environment. Summary of the invention
[0006] In view of this, the object of the present invention is to provide a copper electroplating solution for chip packaging and a preparation method thereof. The present invention uses thiolated chitosan quaternary ammonium salt as a copper electroplating leveler, does not need to be matched with an inhibitor, is non-toxic, environmentally friendly, and the copper electroplating solution prepared by the thiolated chitosan quaternary ammonium salt has a good electroplating effect.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The invention provides application of thiolated chitosan quaternary ammonium salt as a copper electroplating leveler. The thiolated chitosan quaternary ammonium salt is obtained by modifying chitosan with 2,3-epoxypropyltrimethylammonium chloride and N-acetyl-L-cysteine.
[0009] Preferably, the method for preparing the thiolated chitosan quaternary ammonium salt comprises the following steps:
[0010] Chitosan is reacted with 2,3-epoxypropyltrimethylammonium chloride to obtain chitosan quaternary ammonium salt;
[0011] reacting the chitosan quaternary ammonium salt with N-acetyl-L-cysteine to obtain the thiolated chitosan quaternary ammonium salt;
[0012] The deacetylation degree of the chitosan is 87% and the weight average molecular weight is 50 kDa; the mass ratio of the chitosan to 2,3-epoxypropyltrimethylammonium chloride is 1:2.7; and the mass ratio of the chitosan quaternary ammonium salt to N-acetyl-L-cysteine is 1:3.27.
[0013] The present invention provides a copper electroplating solution for chip packaging, comprising the following components:
[0014] Copper sulfate 180-240 g / L, sulfuric acid 45-80 g / L, hydrochloric acid 30-50 ppm, leveler 0.1-1 ppm, accelerator 5-50 ppm, softener 1-5 ppm and water balance, the copper sulfate is calculated as CuSO4, the sulfuric acid is calculated as H2SO4, the hydrochloric acid is calculated as Cl - The leveling agent is the quaternary ammonium salt of thiolated chitosan used in the above technical solution.
[0015] Preferably, the content of the leveler in the copper electroplating solution for chip packaging is 0.5-1 ppm.
[0016] Preferably, the content of the softener in the copper electroplating solution for chip packaging is 2-3 ppm.
[0017] Preferably, the accelerator is one or more of sodium polydisulfide propane sulfonate, sodium 3-mercaptopropane sulfonate and sodium N,N-dimethyl-dithiocarboxamide propane sulfonate.
[0018] Preferably, the softener is N-(3-sulfopropyl)-saccharin sodium salt.
[0019] The present invention provides a method for preparing the copper electroplating solution for chip packaging described in the above technical solution, comprising the following steps:
[0020] Copper sulfate, sulfuric acid, hydrochloric acid, a leveler, an accelerator, a softener and water are mixed to obtain the copper electroplating solution for chip packaging.
[0021] Preferably, the hydrochloric acid is electronic grade hydrochloric acid with a content of 32 wt%.
[0022] Preferably, the sulfuric acid is electronic grade sulfuric acid with a content of 96 wt%.
[0023] The present invention provides the application of thiolated chitosan quaternary ammonium salt as a copper electroplating leveling agent, wherein the thiolated chitosan quaternary ammonium salt is obtained by modifying chitosan by 2,3-epoxypropyltrimethylammonium chloride and N-acetyl-L-cysteine. In the present invention, the thiolated chitosan quaternary ammonium salt has a thiol group, a hydroxypropyltrimethylammonium chloride cation, an N-acetylamino group and an amino structure (-NH-), has a strong adsorption capacity on the Cu surface, and reduces the deposition rate of Cu ions; the N-acetylamino group provides a nitrogen atom with a lone pair of electrons, forms a stable complex with copper ions, and helps to improve the uniformity and smoothness of the electrodeposition process, thereby improving the quality of the coating. Therefore, the thiolated chitosan quaternary ammonium salt has good inhibition and leveling effects as a copper electroplating leveling agent, does not need to be matched with an inhibitor, and is conducive to improving the mechanical properties of narrow line width copper wires; and the thiolated chitosan quaternary ammonium salt is non-toxic, has good biocompatibility, is biodegradable, and is environmentally friendly.
[0024] The present invention provides a copper electroplating solution for chip packaging, comprising the following components: 180-240 g / L of copper sulfate, 45-80 g / L of sulfuric acid, 30-50 ppm of hydrochloric acid, 0.1-1 ppm of leveling agent, 5-50 ppm of accelerator, 1-5 ppm of softener and the balance of water, wherein the copper sulfate is calculated as CuSO4, the sulfuric acid is calculated as H2SO4, and the hydrochloric acid is calculated as Cl - The leveling agent is the thiolated chitosan quaternary ammonium salt in the application described in the above technical solution. The thiolated chitosan quaternary ammonium salt in the copper electroplating solution for chip packaging provided by the present invention has good inhibition and leveling effects, and the electroplating solution does not need to add inhibitors; the present invention adds a softener to the copper electroplating solution to improve the mechanical properties of the copper plating layer and facilitate subsequent processing. The copper electroplating solution for chip packaging provided by the present invention has good electroplating effect, and the plating layer is bright and flat, and there is no obvious defect on the surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the 3D profiler image of the electroplating on the wafer surface of Example 1;
[0026] Figure 2 This is the SEM image of the RDL electroplating circuit on the wafer surface of Example 1;
[0027] Figure 3 This is an ultra-depth-of-field micrograph of the wafer surface of Example 1;
[0028] Figure 4 This is a 3D profiler image of the electroplating on the wafer surface of Example 2;
[0029] Figure 5 This is the SEM image of the RDL electroplating circuit on the wafer surface of Example 2;
[0030] Figure 6 This is an ultra-depth-of-field micrograph of the wafer surface in Example 2;
[0031] Figure 7 This is a 3D profiler image of the electroplating on the wafer surface of Example 3;
[0032] Figure 8 This is the SEM image of the RDL electroplating circuit on the wafer surface of Example 3;
[0033] Fig. 9 This is an ultra-depth-of-field micrograph of the wafer surface of Example 3;
[0034] Fig.10 This is the 3D profiler image of the electroplating on the wafer surface of Comparative Example 1;
[0035] Fig.11 This is the SEM image of the RDL electroplating circuit on the wafer surface of Comparative Example 1;
[0036] Fig.12 This is the ultra-depth-of-field micrograph of the wafer surface of Comparative Example 1;
[0037] Fig.13 This is the 3D profiler image of the electroplating on the wafer surface of Comparative Example 2;
[0038] Fig.14 This is the SEM image of the RDL electroplating circuit on the wafer surface of Comparative Example 2;
[0039] Fig.15 This is an ultra-depth-of-field micrograph of the wafer surface of Comparative Example 2. DETAILED DESCRIPTION
[0040] The invention provides application of thiolated chitosan quaternary ammonium salt as a copper electroplating leveler. The thiolated chitosan quaternary ammonium salt is obtained by modifying chitosan with 2,3-epoxypropyltrimethylammonium chloride and N-acetyl-L-cysteine.
[0041] In the present invention, the preparation method of the thiolated chitosan quaternary ammonium salt preferably comprises the following steps:
[0042] reacting chitosan with 2,3-epoxypropyltrimethylammonium chloride (referred to as the first reaction) to obtain chitosan quaternary ammonium salt;
[0043] The chitosan quaternary ammonium salt is reacted with N-acetyl-L-cysteine (recorded as the second reaction) to obtain the thiolated chitosan quaternary ammonium salt.
[0044] In the present invention, the deacetylation degree of the chitosan is preferably 87%, and the weight average molecular weight is preferably 50 kDa; the mass ratio of the chitosan to 2,3-epoxypropyltrimethylammonium chloride is preferably 1:2.7; the mass ratio of the chitosan quaternary ammonium salt to N-acetyl-L-cysteine is preferably 1:3.27. The present invention has no special requirements for the specific process and reaction conditions of the first reaction and the second reaction, and the preparation process of the thiolated chitosan quaternary ammonium salt (TMC-SH) in the document "Construction, Characterization and In Vitro Evaluation of Cascade Responsive Ternary Gene Complex" (Liu Qing, "Master's Thesis of Shanghai Jiaotong University", 2016, pages 25-27) can be used.
[0045] In the present invention, the thiolated chitosan quaternary ammonium salt has a thiol group, a hydroxypropyltrimethylammonium chloride cation, an N-acetylamino group and an amino structure. While ensuring good water solubility, the thiol group in the thiolated chitosan quaternary ammonium salt enhances the adsorption capacity of the leveler on the copper surface; the N-acetylamino group provides a nitrogen atom with a lone pair of electrons to form a stable complex with copper ions, which helps to improve the uniformity and smoothness of the electrodeposition process, thereby improving the quality of the coating; the hydroxypropyltrimethylammonium chloride cation provides a positively charged nitrogen atom N +The surface tension can also be reduced by adsorbing on the surface of the plating solution. The present invention uses the thiolated chitosan quaternary ammonium salt as a copper electroplating leveling agent, which has good inhibition and leveling effects, does not need to be matched with an inhibitor, and the thiolated chitosan quaternary ammonium salt has good stability and does not react or volatilize with other chemical substances in the electroplating solution, thereby reducing the consumption of additives and extending the life of the electroplating solution; in addition, the thiolated chitosan quaternary ammonium salt is non-toxic, has good biocompatibility, is biodegradable, and is environmentally friendly.
[0046] The present invention provides a copper electroplating solution for chip packaging, comprising the following components:
[0047] Copper sulfate 180-240 g / L, sulfuric acid 45-80 g / L, hydrochloric acid 30-50 ppm, leveler 0.1-1 ppm, accelerator 5-50 ppm, softener 1-5 ppm and water balance, wherein the copper sulfate is calculated as CuSO4, the sulfuric acid is calculated as H2SO4, the hydrochloric acid is calculated as Cl - The leveling agent is the quaternary ammonium salt of thiolated chitosan used in the above technical solution.
[0048] In the present invention, unless otherwise specified, the raw materials involved are commercially available products well known in the art.
[0049] The copper electroplating solution for chip packaging provided by the present invention comprises 180-240 g / L of copper sulfate, preferably 200-240 g / L of copper sulfate, wherein the copper sulfate is calculated as CuSO4.
[0050] The copper electroplating solution for chip packaging provided by the present invention comprises 45 to 80 g / L of sulfuric acid, preferably 60 to 80 g / L of sulfuric acid, wherein the sulfuric acid is calculated as H2SO4.
[0051] The copper electroplating solution for chip packaging provided by the present invention comprises 30 to 50 ppm, preferably 30 to 40 ppm, of hydrochloric acid. - In the present invention, the hydrochloric acid provides chloride ions, which work synergistically with the accelerator to promote the deposition of copper ions.
[0052] The copper electroplating solution for chip packaging provided by the present invention comprises 0.1-1 ppm of a leveling agent, preferably 0.5-1 ppm, and the leveling agent is the quaternary ammonium salt of thiolated chitosan used in the application described in the above technical solution.
[0053] The copper electroplating solution for chip packaging provided by the present invention comprises 5 to 50 ppm, preferably 20 to 30 ppm, of an accelerator. In the present invention, the accelerator is preferably one or more of sodium polydisulfide propane sulfonate (SPS), sodium 3-mercaptopropane sulfonate (MPS) and sodium N,N-dimethyl-dithiocarboxamide propane sulfonate (DPS).
[0054] The copper electroplating solution for chip packaging provided by the present invention comprises 1 to 5 ppm of a softener, preferably 2 to 3 ppm. In the present invention, the softener is preferably N-(3-sulfopropyl)-saccharin sodium salt (SAPS). In the present invention, the softener can improve the mechanical properties of the copper plating layer and facilitate subsequent processing.
[0055] The copper electroplating solution for chip packaging provided by the present invention comprises a water balance.
[0056] The copper electroplating solution for chip packaging provided by the invention has good electroplating effect, and the plating layer is bright and smooth, and the surface has no obvious defects.
[0057] The present invention provides a method for preparing the copper electroplating solution for chip packaging described in the above technical solution, comprising the following steps:
[0058] Copper sulfate, sulfuric acid, hydrochloric acid, a leveler, an accelerator, a softener and water are mixed to obtain the copper electroplating solution for chip packaging.
[0059] In the present invention, the copper sulfate is preferably a superior product in accordance with HG / T 3592-2010 "Copper sulfate for electroplating", the sulfuric acid is preferably 96wt% electronic grade sulfuric acid, and the hydrochloric acid is preferably 32wt% electronic grade hydrochloric acid. In the present invention, the water is preferably ultrapure water.
[0060] In the present invention, the mixing method is preferably:
[0061] The copper sulfate, sulfuric acid, hydrochloric acid and water are first mixed to obtain a base solution;
[0062] A leveling agent, an accelerator and a softener are added to the base liquid for a second mixing to obtain the copper electroplating solution for chip packaging.
[0063] In the present invention, the first mixing and the second mixing are preferably carried out at room temperature. The present invention has no special requirements for the first mixing and the second mixing methods. It is sufficient to use a mixing method well known to those skilled in the art to ensure that the components are mixed evenly.
[0064] In order to further illustrate the present invention, the copper electroplating solution for chip packaging and the preparation method thereof provided by the present invention are described in detail below in conjunction with examples, but they should not be construed as limiting the protection scope of the present invention.
[0065] In various embodiments:
[0066] Copper sulfate is preferably a superior product that complies with HG / T 3592-2010 "Copper sulfate for electroplating";
[0067] The sulfuric acid is electronic grade sulfuric acid with a content of 96 wt%;
[0068] The hydrochloric acid is electronic grade hydrochloric acid with a content of 32wt%;
[0069] The thiolated chitosan quaternary ammonium salt was prepared according to the preparation method of thiolated chitosan quaternary ammonium salt (TMC-SH) in the literature "Construction, characterization and in vitro evaluation of cascade-responsive ternary gene complexes" (Liu Qing, "Master's thesis of Shanghai Jiaotong University", 2016, pages 25-27), as follows:
[0070] (a) Synthesis of Chitosan Quaternary Ammonium Salt (TMC): 2.0 g chitosan (50 kD, deacetylation degree 87%, Zhejiang Jinke Pharmaceutical Co., Ltd.) was added to a 250 mL three-necked round-bottom flask, and 70 mL deionized water (containing 0.5% HAc) was added. The mixture was stirred mechanically at 60 °C for 5 h, heated to 85 °C and stirred for 1 h, and then 20 mL of aqueous solution prepared by 5.4 g 2,3-epoxypropyltrimethylammonium chloride was added in 3 batches, with an interval of 2 h between each batch. The reaction was continued for 12 h. After the reaction was completed, the mixture was filtered, and the filtrate was suspended and evaporated to about 35 mL, and precipitated with a mixed solvent of ethanol / acetone (v / v=1 / 1). The mixture was placed in a fume hood overnight and vacuum dried for 2 days. The mixture was redissolved, dialyzed (MWCO≥3000), and freeze-dried.
[0071] (b) Synthesis of thiolated chitosan quaternary ammonium salt (TMC-SH): Chitosan quaternary ammonium salt (100 mg) was placed in a 25 mL round-bottom flask, and 10 mL of deionized water was added. The mixture was stirred until a transparent solution was formed. EDAC (1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, 767 mg) and NAC (N-acetyl-L-cysteine, 327 mg) were added, and the mixture was stirred for 24 h at room temperature in the dark under nitrogen protection. The reaction solution was taken out and dialyzed (MWCO ≥ 7000) with a 5 mM hydrochloric acid solution containing 0.2% EDTA once, a 5 mM hydrochloric acid solution containing 1% NaCl twice, and a 1 mM hydrochloric acid solution twice at 10°C in the dark within 3 days, and then freeze-dried.
[0072] Example 1
[0073] The copper electroplating solution for chip packaging is prepared by mixing copper sulfate, sulfuric acid, hydrochloric acid, an accelerator, a leveler, a softener and water; the accelerator is sodium polydisulfide propane sulfonate (SPS), the softener is N-(3-sulfopropyl)-saccharin sodium salt (SAPS), and the leveler is thiolated chitosan quaternary ammonium salt; the content of each component in the copper electroplating solution is: CuSO4 240g / L, H2SO4 80g / L, chloride ion 30ppm, accelerator (SPS) 20ppm, softener (SAPS) 3ppm, leveler thiolated chitosan quaternary ammonium salt 1ppm.
[0074] The wafer slices were electroplated at 1ASD for 30 minutes at room temperature. After the filling (including RDL (on-chip wiring) and blind hole filling, the blind hole depth was 87 microns), the profilometer and SEM inspection were performed. The results are as follows Figure 1 , Figure 2 and Figure 3 As shown, Figure 1 This is the 3D profiler image of the wafer surface electroplating. Figure 2 This is the SEM image of the RDL electroplating circuit on the wafer surface. Figure 3 This is an ultra-depth micrograph of the wafer surface. It can be seen that the coating is bright and smooth, with no obvious defects on the surface, and the RDL roughness Ra is 45nm.
[0075] Example 2
[0076] The copper electroplating solution for chip packaging is prepared by mixing copper sulfate, sulfuric acid, hydrochloric acid, an accelerator, a leveler, a softener and water; the accelerator is sodium polydisulfide propane sulfonate (SPS), the softener is N-(3-sulfopropyl)-saccharin sodium salt (SAPS), and the leveler is thiolated chitosan quaternary ammonium salt; the content of each component in the copper electroplating solution is: CuSO4 240g / L, H2SO4 80g / L, chloride ion 30ppm, accelerator (SPS) 20ppm, softener (SAPS) 3ppm, leveler thiolated chitosan quaternary ammonium salt 0.5ppm.
[0077] The wafer slices were electroplated at 1ASD for 30 minutes at room temperature. After the filling was completed, the profilometer and SEM were used for detection. The results are as follows: Figure 4 , Figure 5 and Figure 6 As shown, Figure 4 This is the 3D profiler image of the wafer surface electroplating. Figure 5 This is the SEM image of the RDL electroplating circuit on the wafer surface. Figure 6 This is an ultra-depth-of-field micrograph of the wafer surface. It can be seen that the coating is bright and smooth, with no obvious defects on the surface, and the RDL roughness Ra is 37nm.
[0078] Example 3
[0079] The copper electroplating solution for chip packaging is prepared by mixing copper sulfate, sulfuric acid, hydrochloric acid, an accelerator, a leveler, a softener and water; the accelerator is sodium polydisulfide propane sulfonate (SPS), the softener is N-(3-sulfopropyl)-saccharin sodium salt (SAPS), and the leveler is thiolated chitosan quaternary ammonium salt; the content of each component in the copper electroplating solution is: CuSO4 240g / L, H2SO4 80g / L, chloride ion 30ppm, accelerator (SPS) 20ppm, softener (SAPS) 3ppm, and leveler thiolated chitosan quaternary ammonium salt 0.1ppm.
[0080] The wafer slices were electroplated at 1ASD for 30 minutes at room temperature. After the filling was completed, the profilometer and SEM were used for detection. The results are as follows: Figure 7 , Figure 8 and Fig. 9 As shown, Figure 7 This is the 3D profiler image of the wafer surface electroplating. Figure 8 This is the SEM image of the RDL electroplating circuit on the wafer surface. Fig. 9 It is a super-depth micrograph of the wafer surface. It can be seen that the coating brightness of Example 3 is lower than that of Examples 1 and 2, and the surface is flat and has no obvious defects, and the RDL roughness Ra is 68nm.
[0081] Comparative Example 1
[0082] The copper electroplating solution for chip packaging is prepared by mixing copper sulfate, sulfuric acid, hydrochloric acid, an accelerator, a softener and water; the accelerator is sodium polydisulfide propane sulfonate (SPS), and the softener is N-(3-sulfopropyl)-saccharin sodium salt (SAPS); the content of each component in the copper electroplating solution is: CuSO4 240g / L, H2SO4 80g / L, chloride ion 30ppm, accelerator (SPS) 20ppm, softener (SAPS) 3ppm, and the content of leveling agent thiolated chitosan quaternary ammonium salt is 0ppm.
[0083] The wafer slices were electroplated at 1ASD for 30 minutes. After the filling was completed, the profilometer and SEM were used for testing. The results are as follows: Fig.10 , Fig.11 and Fig.12 As shown, Fig.10 This is the 3D profiler image of the wafer surface electroplating. Fig.11 This is the SEM image of the RDL electroplating circuit on the wafer surface. Fig.12 Ultra-depth micrograph of the wafer surface (with Figure 3 The scale is the same). It can be seen that there are obvious defects on the coating surface, the flatness is low, and the RDL roughness Ra is 180nm.
[0084] Comparative Example 2
[0085] The copper electroplating solution for chip packaging is prepared by mixing copper sulfate, sulfuric acid, hydrochloric acid, an accelerator, a leveler, a softener and water; the accelerator is sodium polydisulfide propane sulfonate (SPS), the softener is N-(3-sulfopropyl)-saccharin sodium salt (SAPS), and the leveler is thiolated chitosan quaternary ammonium salt; the content of each component in the copper electroplating solution is: CuSO4 240g / L, H2SO4 80g / L, chloride ion 30ppm, accelerator (SPS) 20ppm, softener (SAPS) 3ppm, leveler thiolated chitosan quaternary ammonium salt 2ppm.
[0086] The wafer slices were electroplated at 1ASD for 30 minutes. After the filling was completed, the profilometer and SEM were used for testing. The results are as follows: Fig.13 , Fig.14 and Fig.15 As shown, Fig.13 This is the 3D profiler image of the wafer surface electroplating. Fig.14 This is the SEM image of the RDL electroplating circuit on the wafer surface. Fig.15 This is an ultra-depth micrograph of the wafer surface. It can be seen that obvious defects appear on the coating surface, the flatness decreases rapidly, and the RDL roughness Ra is 260nm.
[0087] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A copper electroplating solution for chip packaging, characterized in that: It is composed of the following components: Copper sulfate 180-240 g / L, sulfuric acid 45-80 g / L, hydrochloric acid 30-50 ppm, leveler 0.1-1 ppm, accelerator 5-50 ppm, softener 1-5 ppm and water balance, the copper sulfate is calculated as CuSO4, the sulfuric acid is calculated as H2SO4, the hydrochloric acid is calculated as Cl - The leveling agent is a thiolated chitosan quaternary ammonium salt, which is obtained by modifying chitosan with 2,3-epoxypropyltrimethylammonium chloride and N-acetyl-L-cysteine; the accelerator is one or more of polydisulfide propane sulfonate sodium, 3-mercaptopropane sulfonate sodium salt and N,N-dimethyl-dithiocarboxamide propane sulfonate sodium; the softener is N-(3-sulfopropyl)-saccharin sodium salt; The preparation method of the mercaptolated chitosan quaternary ammonium salt comprises the following steps: Chitosan is reacted with 2,3-epoxypropyltrimethylammonium chloride to obtain chitosan quaternary ammonium salt; reacting the chitosan quaternary ammonium salt with N-acetyl-L-cysteine to obtain the thiolated chitosan quaternary ammonium salt; The deacetylation degree of the chitosan is 87%, and the weight average molecular weight is 50 kDa; the mass ratio of the chitosan to 2,3-epoxypropyltrimethylammonium chloride is 1:2.7; and the mass ratio of the chitosan quaternary ammonium salt to N-acetyl-L-cysteine is 1:3.
27.
2. The copper electroplating solution for chip packaging according to claim 1, characterized in that: The content of the leveling agent in the copper electroplating solution for chip packaging is 0.5-1 ppm.
3. The copper electroplating solution for chip packaging according to claim 1, characterized in that: The content of the softener in the copper electroplating solution for chip packaging is 2-3 ppm.
4. The method for preparing the copper electroplating solution for chip packaging according to any one of claims 1 to 3, characterized in that: The following steps are involved: Copper sulfate, sulfuric acid, hydrochloric acid, a leveler, an accelerator, a softener and water are mixed to obtain the copper electroplating solution for chip packaging.
5. The preparation method according to claim 4, characterized in that: The hydrochloric acid is electronic grade hydrochloric acid with a content of 32 wt %.
6. The preparation method according to claim 4, characterized in that: The sulfuric acid is electronic grade sulfuric acid with a content of 96 wt %.