Inkjet recording method

By applying water-based ink to a non-permeable substrate under conditions where the electrostatic polarity is opposite to that of the ink's Zeta potential, and by using a pretreatment solution and controlling the ink application conditions, the problems of spraying accuracy and timing deviation on non-permeable substrates were solved, achieving high-quality image recording.

CN118302300BActive Publication Date: 2026-11-20FUJIFILM CORP
View PDF 25 Cites 0 Cited by

Patent Information

Application Number
CN202280077793.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-11-25
Filing Date
2022-11-17
Publication Date
2026-11-20
Estimated Expiration
2042-11-17

AI Technical Summary

Technical Problem

When recording images using water-containing inks on non-permeable substrates, quality degradation can easily occur due to decreased jetting accuracy and jetting timing deviations.

Method used

When applying water-containing inks to a non-permeable substrate, the electrostatic polarity of the ink application surface is opposite to the zeta potential polarity of the ink, and the ink application conditions are controlled within a difference range of 30 to 110. A pretreatment solution containing water and a coagulant is used, and colored and white inks are applied to the same surface to ensure that the zeta potential polarity of the inks is consistent.

Benefits of technology

It effectively suppressed the decrease in ink jetting accuracy and jetting timing deviation, thus improving image quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004854251260000341
    Figure GDA0004854251260000341
  • Figure GDA0004854251260000411
    Figure GDA0004854251260000411
  • Figure GDA0004854251260000501
    Figure GDA0004854251260000501
Patent Text Reader

Abstract

An inkjet recording method comprising: an ink-imparting step of imparting an ink containing water to a non-penetrable substrate by an inkjet method, in the ink-imparting step, the ink is imparted to the non-penetrable substrate under a condition that a static polarity of a surface of the non-penetrable substrate to which the ink is imparted is opposite to a polarity of a Zeta potential of the ink.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to an inkjet recording method. Background Technology

[0002] In the past, various studies have been conducted on inkjet recording methods.

[0003] For example, in Patent Document 1, as an inkjet recording medium and inkjet recording method with excellent image density and ink fixing properties, an inkjet recording medium having at least one ink absorption layer on a support having a surface Zeta potential of +5mV or more and +30mV or less at pH 7 on the recording surface, and an inkjet recording method for recording in the inkjet recording medium using a recording liquid with a negative Zeta potential.

[0004] Patent Document 1: Japanese Patent Application Publication No. 2004-291237 Summary of the Invention

[0005] The technical problem to be solved by the invention

[0006] As mentioned above, Patent Document 1 discloses an inkjet recording method for recording images on a recording medium containing an ink absorption layer.

[0007] However, through the research of the inventors, it was determined that when a non-permeable substrate is used as the recording medium instead of the recording medium containing the ink absorption layer, and an image is recorded on the non-permeable substrate using ink containing water, a decrease in quality is likely to occur due to a decrease in ink ejection accuracy and / or ejection timing deviation.

[0008] Here, the decrease in ink ejection accuracy indicates a decrease in the positional accuracy of the ink reaching the non-permeable substrate, and the ink ejection timing deviation indicates a deviation between the timing of the ink reaching the non-permeable substrate and the ideal timing.

[0009] One aspect of the present invention is to provide an inkjet recording method that uses water-containing ink to record images on a non-permeable substrate that suppresses quality degradation caused by decreased ink jetting accuracy and / or jetting timing deviation.

[0010] means for solving technical problems

[0011] The present invention includes the following methods.

[0012] <1> An inkjet recording method, comprising: an ink application step, wherein an ink containing water is applied to a non-permeable substrate by inkjet printing.

[0013] In the ink application process, the ink is applied to the non-permeable substrate under the condition that the electrostatic polarity of the surface on which the ink is applied is opposite to the polarity of the Zeta potential of the ink.

[0014] <2> According to the inkjet recording method described in <1>, in the ink application process, when the electrostatic charge of the surface of the non-permeable substrate to which the ink is applied is set to AkV and the Zeta potential of the ink is set to BmV, the ink is applied to the non-permeable substrate when the difference [AB] obtained by subtracting B from A is 30 to 110.

[0015] <3> According to the inkjet recording method described in <2>, in the ink application process, the ink is applied to the non-permeable substrate under the condition that the difference [AB] is 45 to 70.

[0016] <4> The inkjet recording method according to any one of <1> to <3>, wherein the Zeta potential of the ink is -80mV to -30mV.

[0017] <5> The inkjet recording method according to any one of <1> to <4>, wherein the electrostatic charge on the surface of the non-permeable substrate to which the ink is applied is 10kV to 30kV.

[0018] <6> The inkjet recording method according to any one of <1> to <5>, wherein the non-permeable substrate is a resin substrate.

[0019] <7> The inkjet recording method according to any one of <1> to <6> further includes: a pretreatment solution application step, wherein, prior to the ink application step, a pretreatment solution containing water and a coagulant is applied to the non-permeable substrate.

[0020] In the ink application process, the ink is applied to the area on the non-permeable substrate that has been treated with the pretreatment liquid.

[0021] <8> The inkjet recording method according to any one of <1> to <7>, wherein an ink group comprising at least one coloring ink containing water and coloring pigment and at least one white ink containing water and white pigment is used.

[0022] In the ink application process, under the conditions a1, a2 and a3 below, the at least one colored ink and the at least one white ink are respectively applied to the same surface of the non-permeable substrate by inkjet printing.

[0023] Condition a1…The polarity of the Zeta potential of all inks, including the at least one colored ink and the at least one white ink, is the same.

[0024] Condition a2… The electrostatic polarity of the same side of the non-permeable substrate is opposite to the polarity of the Zeta potential of all the inks.

[0025] Condition a3... When the electrostatic charge of the same side of the non-permeable substrate is set to AkV, and the Zeta potential of each of the at least one colored ink and the at least one white ink is set to BmV, for all the inks, the difference [AB] obtained by subtracting B from A is 30 to 110.

[0026] <9> According to the inkjet recording method described in <8>, among the differences [AB] of the at least one colored ink and the at least one white ink, the difference [AB] of the last ink is the largest.

[0027] <10> According to the inkjet recording method described in <8> or <9>, wherein, when an integer greater than 2 is set as n in the at least one colored ink and the at least one white ink, the difference [AB] of the ink applied in the nth order becomes the same value or greater than the difference [AB] of the ink applied in the (n-1)th order, and the difference [AB] of the last applied ink is greater than the difference [AB] of the first applied ink.

[0028] Invention Effects

[0029] According to one aspect of the present invention, an inkjet recording method is provided that uses water-containing ink to record images on a non-permeable substrate, suppressing quality degradation caused by decreased ink jetting accuracy and / or jetting timing deviation. Detailed Implementation

[0030] In this specification, the numerical range represented by “~” indicates the range included by taking the values ​​before and after “~” as the minimum and maximum values, respectively.

[0031] Within the numerical ranges described in this specification, the upper or lower limit of a certain numerical range can be replaced with the upper or lower limit of other numerical ranges described in different periods. Furthermore, within the numerical ranges described in this specification, the upper or lower limit of a certain numerical range can also be replaced with the values ​​shown in the embodiments.

[0032] In this specification, when multiple substances corresponding to each component are present in the composition, unless otherwise stated, the amount of each component in the composition represents the total amount of the multiple substances present in the composition.

[0033] In this specification, a combination of two or more preferred methods is a more preferred method.

[0034] In this specification, the term "process" includes not only individual processes, but also processes that achieve the desired purpose of the process, even if they cannot be clearly distinguished from other processes.

[0035] In this specification, "image" refers to the entire film formed by ink, and "image recording" refers to the formation of an image (i.e., the film).

[0036] Furthermore, the concept of "image" in this specification also includes solid images.

[0037] In this specification, coloring ink refers to ink of any color other than white, and coloring pigment refers to pigment of any color other than white.

[0038] The concept of coloring inks also includes black inks, and the concept of coloring pigments also includes black pigments.

[0039] In this specification, "(meth)acrylate" is a concept that includes both acrylates and methacrylates.

[0040] "(Meth)acrylic acid" is a concept that includes both acrylic acid and methacrylic acid.

[0041] "alkylene glycols" is a concept that includes both monoalkylene glycols and polyalkylene glycols.

[0042] "alkylene glycol alkyl ethers" is a concept that includes monoalkylene glycol monoalkyl ethers, monoalkylene glycol polyalkyl ethers, polyalkylene glycol monoalkyl ethers, and polyalkylene glycol polyalkyl ethers.

[0043] [Inkjet Recording Method]

[0044] The inkjet recording method of the present invention (hereinafter also simply referred to as the "recording method") includes:

[0045] The ink application process involves applying water-based ink to a non-porous substrate using an inkjet printing method.

[0046] In the ink application process, the ink is applied to the non-permeable substrate under the condition that the electrostatic polarity of the surface on which the ink is applied is opposite to the polarity of the zeta potential of the ink.

[0047] The recording method of the present invention may also include other steps as needed.

[0048] According to the recording method of the present invention, an image is obtained by applying the above-mentioned water-containing ink to a non-permeable substrate. In the obtained image, the quality degradation caused by the decrease in ink jetting accuracy (i.e., the decrease in the positional accuracy of the ink reaching the non-permeable substrate) and / or jetting timing deviation (i.e., the timing of the ink reaching the non-permeable substrate deviates from the ideal timing) is suppressed.

[0049] The reason for suppressing the decrease in ink ejection accuracy using the recording method of the present invention is that the electrostatic polarity of the ink-bearing surface of the non-permeable substrate is opposite to the polarity of the ink's zeta potential, generating an attraction between the ink-bearing surface of the non-permeable substrate and the ink. This attraction improves the straightness of the ink, thereby improving the ink ejection accuracy.

[0050] Furthermore, it is believed that the aforementioned gravity also helps to suppress jet timing deviation.

[0051] The following describes each step of the recording method of the present invention.

[0052] <Ink application process>

[0053] The ink application process is a process of applying water-containing ink to a non-permeable substrate by inkjet printing, and the ink is applied to the non-permeable substrate under the condition that the electrostatic polarity of the surface of the non-permeable substrate to which the ink is applied is opposite to the polarity of the zeta potential of the ink.

[0054] (Non-permeable substrate)

[0055] In the ink application process, the above-mentioned ink is applied to a non-permeable substrate.

[0056] In this invention, non-permeable substrate refers to a substrate with a water absorption rate (mass %, 24 hours) of less than 0.2 according to ASTM D570 of the ASTM test method.

[0057] There are no particular limitations on the non-permeable substrate, but a resin substrate is preferred.

[0058] There are no particular limitations on the resin substrate; for example, thermoplastic resin substrates can be cited.

[0059] As a resin substrate, examples include substrates in which thermoplastic resin is molded into sheets or films.

[0060] As the resin substrate, a substrate comprising polypropylene, polyethylene terephthalate, nylon, polyethylene or polyimide is preferred.

[0061] The resin substrate can be a transparent resin substrate.

[0062] Here, "transparent" means that the transmittance of visible light with wavelengths of 400 nm to 700 nm is 80% or more (preferably 90% or more).

[0063] As described later in Embodiment 201, in an embodiment where a coloring ink having a hue other than white (preferably colored or black, such as cyan, magenta, yellow, black, etc.) and a white ink with a white hue are sequentially applied to a non-permeable substrate, in the case where the non-permeable substrate is a transparent resin substrate, the coloring image with a white image as a background can be identified from the non-image recording surface (i.e., the surface where no image is recorded) of the non-permeable substrate.

[0064] The resin substrate can be colored.

[0065] The shape of the resin substrate is not particularly limited, but a sheet-like resin substrate is preferred. From the viewpoint of the productivity of the recorded medium, a sheet-like resin substrate that can be rolled into a roll is more preferred.

[0066] The thickness of the resin substrate is preferably 10 μm to 200 μm, and more preferably 10 μm to 100 μm.

[0067] From the perspective of improving surface energy, resin substrates can also undergo surface treatment.

[0068] Examples of surface treatments include corona treatment, plasma treatment, flame treatment, heat treatment, abrasion treatment, and light irradiation treatment (UV treatment), but these are not the only ones that can be mentioned.

[0069] (Ink)

[0070] In the ink application process, water-containing ink is applied to a non-permeable substrate.

[0071] -water-

[0072] The ink contains water.

[0073] The water content relative to the total amount of ink is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more.

[0074] The upper limit of water content depends on the amount of other components, but is preferably 90% by mass or less, more preferably 80% by mass or less, relative to the total amount of ink.

[0075] -pigment-

[0076] Ink can contain at least one pigment.

[0077] As a pigment, there are no particular restrictions; it can be either an organic pigment or an inorganic pigment.

[0078] Examples of organic pigments include, for example, azo pigments, polycyclic pigments (such as phthalocyanine pigments, perylene pigments, violet ketone pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, diketopyrrolopyrrole pigments, thioindole ketone pigments, isoindolinetone pigments, quinolinetone pigments, etc.), dye chelates, nitro pigments, nitroso pigments, aniline black, etc.

[0079] Examples of inorganic pigments include, for example, white inorganic pigments, iron oxide, barium yellow, cadmium red, chrome yellow, and carbon black. Preferred methods for white inorganic pigments will be described later.

[0080] As for pigments, examples include those described in paragraphs 0096 to 0100 of Japanese Patent Application Publication No. 2009-241586.

[0081] Inks containing colored pigments or black pigments can be used as coloring inks (e.g., cyan ink, magenta ink, yellow ink, black ink, etc.).

[0082] Inks containing white pigments (e.g., white inorganic pigments) can be used as white inks (hereinafter also referred to as "white inks").

[0083] Examples of white inorganic pigments include titanium dioxide (TiO2), barium sulfate, calcium carbonate, aluminum hydroxide, silicon dioxide, zinc oxide, zinc sulfide, mica, talc, and pearl. Among white inorganic pigments, titanium dioxide, barium sulfate, calcium carbonate, or zinc oxide are preferred, with titanium dioxide being more preferred.

[0084] The average primary particle size of white inorganic pigments is, for example, 150 nm to 400 nm.

[0085] If the average primary particle size is above 150 nm, the concealment is further improved. Here, concealment refers to the property of covering the substrate by an image (e.g., a white image).

[0086] If the average single-pass particle size is below 400nm, the ink ejectibility is further improved.

[0087] The average primary particle size of the white inorganic pigment is preferably 250 nm to 350 nm, and more preferably 250 nm to 300 nm.

[0088] The average primary particle size of the white inorganic pigment was determined using a transmission electron microscope (TEM). The TEM 1200EX, manufactured by JEOL Co., Ltd., was used for the measurement.

[0089] Specifically, after ink diluted 1,000 times was dropped onto a Cu200 mesh (manufactured by JEOL Ltd.) with a carbon film and dried, the circular equivalent diameter of 300 non-overlapping and independent particles was determined based on an image magnified 100,000 times by TEM, and the value obtained by simply averaging the obtained measurements was taken as the average primary particle size.

[0090] The pigment content, relative to the total amount of ink, is preferably 1% to 20% by mass, more preferably 1% to 15% by mass, and even more preferably 1% to 10% by mass.

[0091] -Resin-

[0092] Ink may contain at least one resin.

[0093] There are no particular limitations on the resin used, but acrylic resin, polyester resin, polyurethane resin or polyolefin resin are preferred.

[0094] The resin content relative to the total amount of ink is preferably 1% to 30% by mass, more preferably 2% to 20% by mass, even more preferably 2% to 15% by mass, and even more preferably 2% to 10% by mass.

[0095] Specifically, examples of resins include pigment dispersion resins used to disperse pigments, and resin particles, which are composed of resins.

[0096] -Pigment Dispersion Resin-

[0097] The resin can contain pigment dispersing resin as a pigment dispersant.

[0098] When the resin contains a pigment dispersion resin, the ink contains a resin-coated pigment having a structure in which at least a portion of the surface of the pigment is coated by the pigment dispersion resin.

[0099] Water-insoluble resins are preferred as pigment dispersion resins.

[0100] Acrylic resins are preferred as pigment dispersion resins.

[0101] Examples of pigment dispersion resins include those described in International Patent Publication No. 2013 / 180074, Japanese Patent No. 5863600, Japanese Unexamined Patent Publication No. 2018-28080, Japanese Unexamined Patent Publication No. 2017-149906, and Japanese Unexamined Patent Publication No. 2016-193981. Pigment dispersion resins are also called "resin dispersants," etc.

[0102] Furthermore, as a combination of pigment and pigment dispersion resin, resin-coated pigments, such as those described in Japanese Patent No. 5404669, in which the pigment is coated with a crosslinked water-soluble resin, can be used. In this case, the resin-coated pigment can be manufactured using, for example, an acrylic resin having carboxyl groups as the water-soluble resin and an epoxy compound with two or more functions as the crosslinking agent.

[0103] From the viewpoint of the adsorption properties of pigments, pigment dispersion resins preferably contain alicyclic or aromatic ring structures, more preferably aromatic ring structures.

[0104] As an alicyclic structure, an alicyclic hydrocarbon structure with 5 to 10 carbon atoms is preferred, and cyclohexane ring structure, dicyclopentanyl ring structure, dicyclopentenyl ring structure, norbornene ring structure, isobornene ring structure, norbornene ring structure, isobornene ring structure, or adamantane ring structure are more preferred.

[0105] As an aromatic ring structure, naphthalene ring or benzene ring is preferred, and benzene ring is more preferred.

[0106] The amount of alicyclic or aromatic ring structure is preferably 0.01 mol to 1.5 mol, more preferably 0.1 mol to 1 mol, relative to 100 g of resin contained in the resin particles.

[0107] From the viewpoint of pigment dispersion performance, pigment dispersion resins preferably have ionic groups in their structure.

[0108] As an ionic group, it can be either an anionic group or a cationic group, but an anionic group is preferred.

[0109] There are no particular limitations on the anionic group, but carboxyl groups, salts of carboxyl groups, sulfonyl groups, or salts of sulfonyl groups are preferred.

[0110] From the viewpoint of pigment dispersibility and storage stability, the acid value of the pigment dispersion resin is preferably 30 mg KOH / g to 300 mg KOH / g, more preferably 30 mg KOH / g to 200 mg KOH / g, and even more preferably 50 mg KOH / g to 200 mg KOH / g.

[0111] Here, the acid value is defined by the mass (mg) of KOH required to fully neutralize 1g of resin, and is determined by the method described in JIS standard (JISK 0070, 1992).

[0112] The weight-average molecular weight (Mw) of the pigment dispersion resin is preferably 30,000 or more, more preferably 30,000 to 150,000, even more preferably 30,000 to 100,000, and even more preferably 30,000 to 80,000.

[0113] When the resin contains a pigment dispersion resin, the content of the pigment dispersion resin relative to the total amount of ink is preferably 1% to 25% by mass, more preferably 1% to 20% by mass, even more preferably 1% to 15% by mass, and even more preferably 1% to 10% by mass.

[0114] When the resin contains a pigment dispersion resin, the ratio of pigment dispersion resin (D) to pigment (P) (i.e., D / P ratio) is preferably 0.05 to 3, more preferably 0.05 to 2, even more preferably 0.05 to 1, and even more preferably 0.05 to 0.7.

[0115] As a dispersing device for dispersing pigments, known dispersing devices can be used, such as ball mills, sand mills, bead mills, roller mills, spray mills, paint mixers, grinders, ultrasonic dispersers, and dispersers.

[0116] There are no particular limitations on the way the pigment is dispersed in the resin. It can be any of the random polymer, block polymer, and graft polymer, and it can be a polymer with a cross-linked structure.

[0117] Pigment dispersion resins are preferably polymers or block polymers with cross-linked structures.

[0118] The following shows preferred embodiments of cross-linked polymers and block polymers as preferred pigment dispersion resins.

[0119] In this invention, polymer refers to a compound with a weight-average molecular weight of 1000 or more.

[0120] In this invention, the weight-average molecular weight is expressed as the value obtained by gel permeation chromatography (GPC). When performing the determination by GPC, an HLC-8020GPC (manufactured by Tosoh Corporation) was used as the measuring apparatus, three TSKgel Super Multipore HZ-H (4.6mm ID × 15cm, manufactured by Tosoh Corporation) columns were used as the column, and THF (tetrahydrofuran) was used as the eluent. Furthermore, the determination was performed using an RI detector, with the sample concentration set to 0.45% by mass, the flow rate set to 0.35 ml / min, the sample injection volume set to 10 μl, and the measurement temperature set to 40°C. The calibration curves were prepared based on eight samples manufactured by Tosoh Corporation: “TSKstandard, polystyrene”, namely “F-40”, “F-20”, “F-4”, “F-1”, “A-5000”, “A-2500”, “A-1000” and “n-propylbenzene”.

[0121] --Polymers with cross-linked structures--

[0122] There are no particular limitations on polymers with cross-linked structures, as long as they have at least one cross-linked structure within the molecule.

[0123] Whether the polymer contained in the ink has a cross-linked structure can be determined, for example, by the following methods. First, the polymer in the ink is separated using separation methods such as solvent extraction. Then, by analyzing the separated polymer using various analytical methods such as nuclear magnetic resonance (NMR), infrared spectroscopy (IR), and thermal analysis, the presence or absence of a cross-linked structure can be comprehensively determined.

[0124] A polymer having a cross-linked structure (hereinafter also referred to as a "cross-linked polymer") is formed, for example, by cross-linking an uncross-linked polymer (hereinafter also referred to as a "non-cross-linked polymer") with a cross-linking agent. The non-cross-linked polymer is preferably a water-soluble polymer.

[0125] In this invention, "water solubility" refers to the property of dissolving 1g or more in 100g of water at 25°C. Preferably, "water solubility" refers to the property of dissolving 3g or more (more preferably 10g or more) in 100g of water at 25°C.

[0126] Furthermore, even if the uncrosslinked polymer is water-soluble, the crosslinked polymer is not necessarily water-soluble.

[0127] Examples of uncrosslinked polymers include vinyl resins, acrylic resins, urethane resins, and polyester resins. Among these, acrylic resins are preferred as the uncrosslinked polymer.

[0128] The uncrosslinked polymer is preferably a polymer having functional groups that can be crosslinked by a crosslinking agent. Examples of crosslinkable functional groups include carboxyl groups or salts thereof, isocyanate groups, and epoxy groups. From the viewpoint of improving pigment dispersibility, the crosslinkable functional group is preferably a carboxyl group or a salt thereof, and particularly preferably a carboxyl group. That is, the uncrosslinked polymer is preferably a polymer containing a carboxyl group.

[0129] The uncrosslinked polymer is preferably a copolymer containing structural units derived from carboxyl-containing monomers (hereinafter referred to as "carboxyl-containing monomers"). The copolymer may contain only one type of structural unit derived from carboxyl-containing monomers or more than two types. The copolymer may be a random copolymer or a block copolymer, but a random copolymer is preferred.

[0130] Examples of carboxyl-containing monomers include (meth)acrylic acid, β-carboxyethyl acrylate, fumaric acid, itaconic acid, maleic acid, and crotonic acid.

[0131] From the viewpoint of crosslinking and dispersibility, the carboxyl-containing monomer is preferably (meth)acrylic acid or β-carboxyethyl acrylate, and more preferably (meth)acrylic acid.

[0132] The content of structural units derived from carboxyl-containing monomers relative to the total amount of uncrosslinked polymer is preferably 5% to 40% by mass, more preferably 10% to 35% by mass, and even more preferably 10% to 30% by mass.

[0133] In addition to structural units derived from carboxyl-containing monomers, the uncrosslinked polymer preferably contains structural units derived from hydrophobic monomers. The copolymer may contain only one type of structural unit derived from hydrophobic monomers, or it may contain two or more types.

[0134] Examples of hydrophobic monomers include (meth)acrylates having alkyl groups having 1 to 20 carbon atoms, (meth)acrylates having aromatic rings (e.g., benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, etc.), styrene, and styrene derivatives.

[0135] The content of structural units derived from hydrophobic monomers relative to the total amount of uncrosslinked polymer is preferably 60% to 95% by mass, more preferably 65% ​​to 90% by mass, and even more preferably 70% to 90% by mass.

[0136] The uncrosslinked polymer is preferably a random copolymer comprising at least one of structural units derived from a carboxyl-containing monomer, structural units derived from an alkyl group having 1 to 20 carbon atoms, and structural units derived from an aromatic ring (meth)acrylate. More preferably, it is a random copolymer comprising structural units derived from (meth)acrylic acid and structural units derived from an aromatic ring (meth)acrylate. Even more preferably, it is a copolymer comprising structural units derived from (meth)acrylic acid and structural units derived from benzyl (meth)acrylate.

[0137] There is no particular limitation on the weight-average molecular weight (Mw) of the uncrosslinked polymer, but from the viewpoint of dispersibility of white pigment, it is preferably 3,000 to 300,000, more preferably 5,000 to 200,000, and even more preferably 7,000 to 100,000.

[0138] The preferred range of weight-average molecular weight for cross-linked polymers is the same as that for uncross-linked polymers.

[0139] When crosslinking uncrosslinked polymers, the crosslinking agent used is preferably a compound having two or more reaction sites with the uncrosslinked polymer (e.g., a polymer with carboxyl groups). Only one crosslinking agent may be used, or two or more may be used.

[0140] A preferred combination of a crosslinking agent and an uncrosslinked polymer is a combination of a compound having two or more epoxy groups (i.e., an epoxy compound with two or more functional groups) and a polymer having carboxyl groups. In this combination, a crosslinked structure is formed by the reaction of epoxy groups and carboxyl groups. The formation of the crosslinked structure using the crosslinking agent is preferably carried out after dispersing the pigment using the uncrosslinked polymer.

[0141] Examples of epoxide compounds with two or more functions include, for example, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, diethylene glycol diglycidyl ether, dipropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, and trimethylolpropane triglycidyl ether.

[0142] Among them, the epoxy compound with two or more functions is preferably polyethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, or trimethylolpropane triglycidyl ether.

[0143] Crosslinking agents can be commercially available products.

[0144] Commercially available products include, for example, Denacol EX-321, EX-821, EX-830, EX-850 and EX-851 (manufactured by Nagase ChemteX Corporation).

[0145] From the viewpoint of crosslinking reaction rate and dispersion stability after crosslinking, the molar ratio of the reactive site (e.g., epoxy group) in the crosslinking agent to the reactive site (e.g., carboxyl group) in the uncrosslinked polymer is preferably 1:1.1 to 1:10, more preferably 1:1.1 to 1:5, and even more preferably 1:1.1 to 1:3.

[0146] --Block Polymer---

[0147] Block polymers, also known as block copolymers, are copolymers in which at least two polymers are bonded together in the molecule.

[0148] The block polymer preferably comprises structural units derived from hydrophobic monomers and structural units derived from monomers containing anionic groups (hereinafter "monomers containing anionic groups").

[0149] Block polymers may contain only one or more structural units derived from hydrophobic monomers. Block polymers may also contain only one or more structural units derived from anionic monomers.

[0150] Examples of structural units derived from hydrophobic monomers include olefinic unsaturated compounds with aromatic or alicyclic structures and (meth)acrylates with alkyl groups having 1 to 20 carbon atoms.

[0151] The content of structural units derived from hydrophobic monomers relative to the total amount of block polymer is preferably 35% to 95% by mass, more preferably 50% to 95% by mass, and even more preferably 70% to 90% by mass.

[0152] From the viewpoint of pigment adsorption, the hydrophobic monomer preferably contains an olefin unsaturated compound having an aromatic ring structure or an alicyclic structure, more preferably an olefin unsaturated compound having an alicyclic structure, and even more preferably an olefin unsaturated compound having an alicyclic structure having 6 or more carbon atoms.

[0153] The content of structural units derived from olefinic unsaturated compounds having aromatic or alicyclic structures relative to the total amount of the block polymer is preferably 10% to 90% by mass, more preferably 20% to 80% by mass, further preferably 30% to 70% by mass, and even more preferably 30% to 60% by mass.

[0154] The structural unit derived from the hydrophobic monomer preferably comprises a (meth)acrylate having an alkyl group having 1 to 20 carbon atoms. The alkyl group can be either linear or branched.

[0155] Examples of (meth)acrylates having alkyl groups having 1 to 20 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and octyl (meth)acrylate.

[0156] The content of structural units derived from (meth)acrylates having alkyl groups having 1 to 20 carbon atoms relative to the total amount of the block polymer is preferably 10% to 90% by mass, more preferably 20% to 80% by mass, further preferably 30% to 70% by mass, and especially preferably 40% to 60% by mass.

[0157] In structural units derived from monomers containing anionic groups, anionic groups can be, for example, carboxyl groups, salts of carboxyl groups, sulfonyl groups, salts of sulfonyl groups, phosphate groups, salts of phosphate groups, phosphonic acid groups, and salts of phosphonic acid groups.

[0158] As counterions in salts, examples include alkali metal ions such as sodium, potassium, and lithium ions; alkaline earth metal ions such as calcium and magnesium ions; and ammonium ions.

[0159] The anionic group is preferably a carboxyl group or a salt of a carboxyl group. Examples of monomers containing anionic groups include (meth)acrylic acid, β-carboxyethyl acrylate, fumaric acid, itaconic acid, maleic acid, and crotonic acid. Among these, (meth)acrylic acid is preferred.

[0160] The content of structural units derived from anionic monomers relative to the total amount of the block polymer is preferably 1% to 30% by mass, more preferably 2% to 25% by mass, and even more preferably 3% to 20% by mass.

[0161] Whether the polymer contained in the ink is a block polymer can be determined, for example, by the following methods. First, the polymer in the ink is separated using separation methods such as solvent extraction. The separated polymer is then analyzed using various analytical methods such as nuclear magnetic resonance (NMR), infrared spectroscopy (IR), and thermal analysis, and its physical properties, such as glass transition temperature, are measured. This comprehensive method allows for a determination of whether the polymer is a block polymer.

[0162] There is no particular limitation on the weight-average molecular weight (Mw) of the block polymer, but from the viewpoint of pigment dispersibility, it is preferably 3,000 to 100,000, more preferably 5,000 to 80,000, and even more preferably 10,000 to 60,000.

[0163] -Resin particles-

[0164] Resins can contain resin particles.

[0165] Here, the difference between resin particles and the pigment dispersion resin mentioned above is that resin particles are composed of resin.

[0166] Water-insoluble resins are preferred as the resins constituting the resin particles.

[0167] There are no particular limitations on the glass transition temperature of the resin particles (i.e., the glass transition temperature of the resin in the resin particles).

[0168] From the viewpoint of further improving image intensity, the glass transition temperature (Tg) of the resin particles is preferably 20°C or higher, more preferably 50°C or higher, and even more preferably 80°C or higher.

[0169] From the viewpoint of suitability for manufacturing resin particles, the glass transition temperature (Tg) of the resin particles is preferably 150°C or less, and more preferably 130°C or less.

[0170] As resin particles, particles made of acrylic resin (hereinafter also referred to as acrylic resin particles), particles made of styrene acrylic resin (hereinafter also referred to as styrene acrylic resin particles), particles made of polyester resin (hereinafter also referred to as polyester resin particles), particles made of polyurethane resin (hereinafter also referred to as polyurethane resin particles), or particles made of polyolefin resin (hereinafter also referred to as polyolefin resin particles) are preferred.

[0171] Self-dispersible resin particles are preferred as resin particles.

[0172] Examples of self-dispersible resin particles include, for instance, those described in Japanese Patent Application Publication No. 2016-188345, paragraphs 0062 to 0076, and International Publication No. 2013 / 180074, paragraphs 0109 to 0140.

[0173] The molecular weight of the resin in the resin particles, measured by weight-average molecular weight, is preferably 10 million to 300,000, more preferably 20 million to 200,000, and even more preferably 50 million to 100,000.

[0174] Weight-average molecular weight was determined by gel permeation chromatography (GPC). Details of GPC are as described above.

[0175] The volume average particle size of the resin particles is preferably 1 nm to 200 nm, more preferably 3 nm to 200 nm, and even more preferably 5 nm to 50 nm.

[0176] When the ink contains resin particles, the content of resin particles relative to the total amount of ink is preferably 1% to 25% by mass, more preferably 2% to 20% by mass, even more preferably 2% to 15% by mass, and even more preferably 2% to 10% by mass.

[0177] Water-soluble organic solvents with boiling points below 220°C-

[0178] The ink preferably contains at least one water-soluble organic solvent with a boiling point below 220°C.

[0179] As a result, the lamination strength of the image recording is further improved.

[0180] In this invention, boiling point refers to the boiling point at 1 atmosphere (101325 Pa).

[0181] Examples of water-soluble organic solvents with boiling points below 220°C include 1,2-propanediol (also known as propylene glycol) (boiling point 188°C), 1,3-propanediol (boiling point 213°C), propylene glycol monomethyl ether (boiling point 121°C), ethylene glycol (boiling point 197°C), ethylene glycol monomethyl ether (boiling point 124°C), propylene glycol monoethyl ether (boiling point 133°C), ethylene glycol monoethyl ether (boiling point 135°C), and propylene glycol. Monopropyl ether (boiling point 149℃), ethylene glycol monopropyl ether (boiling point 151℃), propylene glycol monobutyl ether (boiling point 170℃), ethylene glycol monobutyl ether (boiling point 171℃), 2-ethyl-1-hexanol (boiling point 187℃), dipropylene glycol monomethyl ether (boiling point 188℃), diethylene glycol dimethyl ether (boiling point 162℃), diethylene glycol diethyl ether (boiling point 188℃), dipropylene glycol dimethyl ether (boiling point 175℃), etc.

[0182] When the ink contains a water-soluble organic solvent with a boiling point below 220°C, the content of the water-soluble organic solvent with a boiling point below 220°C relative to the total amount of ink is preferably 1% to 50% by mass, more preferably 5% to 40% by mass, even more preferably 10% to 40% by mass, and even more preferably 15% to 35% by mass.

[0183] Organic solvents with a boiling point above 220°C

[0184] The content of organic solvents with a boiling point of 220°C or higher (hereinafter also referred to as "high-boiling-point solvents") in the ink is preferably 5% by mass or less. This further improves the lamination strength of the image recorder and the adhesion of the image.

[0185] Here, "the content of organic solvents with a boiling point of 220°C or higher in the ink is 5% by mass or less" means that, in the case where the ink does not contain organic solvents with a boiling point of 220°C or higher (i.e., the content of organic solvents with a boiling point of 220°C or higher in the ink is 0% by mass) or contains organic solvents with a boiling point of 220°C or higher, the content of organic solvents with a boiling point of 220°C or higher relative to the total amount of ink is also 5% by mass or less.

[0186] The content of organic solvents with a boiling point of 220°C or higher in the ink is more preferably 3% by mass or less, more preferably 2% by mass or less, more preferably 1% by mass or less, and more preferably 0% by mass.

[0187] Examples of organic solvents with boiling points above 220°C include glycerol (boiling point 290°C), 1,2-hexanediol (HDO) (boiling point 223°C), diethylene glycol (boiling point 245°C), diethylene glycol monobutyl ether (boiling point 230°C), triethylene glycol (boiling point 285°C), dipropylene glycol (boiling point 232°C), tripropylene glycol (boiling point 267°C), trimethylolpropane (boiling point 295°C), 2-pyrrolidone (boiling point 245°C), tripropylene glycol monomethyl ether (boiling point 243°C), and triethylene glycol monomethyl ether (boiling point 248°C).

[0188] -surfactant-

[0189] Ink may contain at least one surfactant.

[0190] Examples of surfactants include nonionic surfactants, cationic surfactants, anionic surfactants, and betaine surfactants.

[0191] As a preferred surfactant, one example of a nonionic surfactant is the acetylene glycol-based surfactant.

[0192] As an acetylene glycol-based surfactant, for example, the acetylene glycol-based surfactant described in paragraphs 0070 to 0080 of International Publication No. 2017 / 149917 can be used.

[0193] Examples of acetylene glycol surfactants include:

[0194] Polyalkylene adducts (preferably polyethylene oxide adducts) of 2,4,7,9-tetramethyl-5-decyn-4,7-diol

[0195] Polyalkylene oxide adducts (preferably polyethylene oxide adducts) of 3,6-dimethyl-4-octyne-3,6-diol

[0196] Polyalkylene adducts (preferably polyethylene oxide adducts) of 2,5,8,11-tetramethyl-6-dodecyne-5,8-diol

[0197] Polyalkylene adduct of 2,5-dimethyl-3-hexyne-2,5-diol (preferably a polyoxyethylene adduct)

[0198] wait.

[0199] Commercially available acetylene glycol surfactants include the Surfynol series (e.g., Surfynol 420, Surfynol 440, Surfynol 465, Surfynol 485), Olfine series (e.g., Olfine E1010, Olfine E1020), and Dynol series (e.g., Dynol 604) manufactured by Air Products Ltd. or Nissin Chemical Co., Ltd.; and ACETYLENOL manufactured by Kawaken Fine Chemicals Co., Ltd., etc.

[0200] Commercially available acetylene glycol surfactants are also supplied by companies such as The Dow Chemical Company and General Aniline & Film Corp.

[0201] Compounds cited as surfactants in Japanese Patent Application Publication No. 59-157636 (pages 37-38) and Research Disclosure No. 308119 (1989) can also be cited. Furthermore, fluorinated (fluoroalkyl) surfactants and ketone surfactants described in Japanese Patent Application Publication Nos. 2003-322926, 2004-325707, and 2004-309806 can also be cited.

[0202] When the ink contains surfactants, the surfactant content in the ink can be adjusted appropriately, taking into account the surface tension of the ink.

[0203] The surfactant content in the ink is preferably 0.01% to 5% by mass relative to the total amount of ink, more preferably 0.05% to 3% by mass, and even more preferably 0.1% to 2% by mass.

[0204] -Other ingredients-

[0205] Ink may contain other ingredients besides those mentioned above.

[0206] Other ingredients include, for example, known additives such as silica compounds (e.g., silica compounds described in paragraphs 0058 to 0075 of Japanese Patent No. 5430316), urea, urea derivatives, waxes, anti-fading agents, emulsion stabilizers, penetration enhancers, ultraviolet absorbers, preservatives, antifungal agents, pH adjusters, defoamers, viscosity modifiers, dispersion stabilizers, and chelating agents.

[0207] -Optimal physical properties of ink-

[0208] The viscosity of the ink (at 25°C) is preferably 1.2 mPa·s or more and 15.0 mPa·s or less, more preferably 2 mPa·s or more and less than 13 mPa·s, and even more preferably 2.5 mPa·s or more and less than 10 mPa·s.

[0209] The surface tension of the ink (at 25°C) is preferably 25mN / m to 50mN / m, more preferably 30mN / m to 45mN / m, and even more preferably 30mN / m to 40mN / m.

[0210] The ink has a pH of 6 to 11 at 25°C, more preferably 7 to 10, and even more preferably 7 to 9.

[0211] The pH of the ink at 25°C was measured using a commercially available pH meter.

[0212] (The effect of ink)

[0213] In the ink application process, the ink is applied to a non-permeable substrate by inkjet printing (i.e., ejected from an inkjet head).

[0214] There are no particular restrictions on the way ink is ejected in inkjet printing. It can be any of the known methods, such as charge control method that uses electrostatic induction to eject ink; on-demand inkjet method (pressure pulse method) that uses the vibration pressure of piezoelectric elements; acoustic inkjet method that converts electrical signals into sound beams to irradiate ink and eject ink using radiation pressure; and thermal inkjet method (Bubble Jet (registered trademark)) that heats ink to form bubbles and uses the resulting pressure.

[0215] As an inkjet method, the inkjet method described in Japanese Patent Application Publication No. 54-59936 can be used in particular, that is, the ink under the action of heat energy will produce a rapid volume change, and the ink will be ejected from the nozzle by the force generated by the change of state.

[0216] As an inkjet method, the method described in paragraphs 0093 to 0105 of Japanese Patent Application Publication No. 2003-306623 may also be applied.

[0217] Ink application based on inkjet technology is achieved by ejecting ink from the nozzles of an inkjet head.

[0218] As inkjet head types, there are reciprocating methods that record while scanning the width of the recorded medium with a short serial printhead, and linear methods that use a line head with recording elements arranged corresponding to the entire area of ​​one side of the recorded medium.

[0219] In the inline method, the recording medium is scanned in a direction intersecting the arrangement direction of the recording elements, enabling image recording across the entire surface of the medium. The inline method eliminates the need for a transport system such as a carriage that scans short nozzles, as required in the reciprocating method. Furthermore, compared to the reciprocating method, the inline method eliminates the need for carriage movement and complex scanning control of the recording medium; only the recording medium is moved. Therefore, the inline method increases image recording speed compared to the reciprocating method.

[0220] The ink is preferably applied using an inkjet head with a resolution of 300 dpi or higher (more preferably 600 dpi, and even more preferably 800 dpi). Here, dpi is an abbreviation for dots per inch, where 1 inch is 2.54 cm.

[0221] From the viewpoint of obtaining high-definition images, the amount of ink droplets ejected from the nozzle of the inkjet head is preferably 1 pL (picoliter) to 10 pL, more preferably 1.5 pL to 6 pL.

[0222] Furthermore, from the perspective of improving image uniformity and the connection of continuous gray levels, combining different droplet volumes is also effective.

[0223] The recording method of the present invention may include a step of preheating a non-permeable substrate prior to an ink application step. In this case, ink is applied to the preheated non-permeable substrate during the ink application step.

[0224] The heating temperature for preheating can be set appropriately, but it is preferable to set the temperature of the non-permeable substrate to 20°C to 50°C, and more preferably to 25°C to 40°C.

[0225] In the ink application process, two or more inks can be applied to a non-permeable substrate.

[0226] As two or more inks, inks of two or more colors are preferred, inks of two or more colors are more preferred, inks of two or more colors are selected from the group consisting of at least one coloring ink and at least one white ink, and inks of two or more colors are even more preferred as a combination of at least one coloring ink and at least one white ink.

[0227] In this invention, coloring ink refers to inks having a color hue other than white (e.g., colored and black) (e.g., cyan ink, magenta ink, yellow ink, and black ink).

[0228] In the ink application process, when two or more colors of ink are sequentially applied to a non-porous substrate...

[0229] An ink of the nth color (n is an integer greater than or equal to 1) can be applied to a non-permeable substrate by heat drying, and an ink of the (n+1)th color can be applied to the ink of the nth color after heat drying.

[0230] Alternatively, the ink of the nth color can be applied to a non-permeable substrate without heating and drying, or the ink of the (n+1)th color can be applied to the ink of the nth color.

[0231] (Static electricity of non-permeable substrates and zeta potential of ink)

[0232] In the ink application process, ink is applied to the non-permeable substrate under conditions where the electrostatic polarity of the surface on which the ink is applied is opposite to the polarity of the Zeta potential of the ink.

[0233] The combination of the above-mentioned electrostatic polarity and the polarity of the above-mentioned Zeta potential can be a combination in which the above-mentioned electrostatic polarity is positive (+) and the polarity of the above-mentioned Zeta potential is negative (-), or it can be a combination in which the above-mentioned electrostatic polarity is negative (-) and the polarity of the above-mentioned Zeta potential is positive (+). However, from the viewpoint of further suppressing the degradation of image quality, the combination in which the above-mentioned electrostatic polarity is positive (+) and the polarity of the above-mentioned Zeta potential is negative (-) is preferred.

[0234] From the viewpoint of further suppressing image quality degradation, the ink application process preferably involves applying ink to the non-permeable substrate when the electrostatic charge of the ink-applied surface of the non-permeable substrate is set to AkV and the Zeta potential of the ink is set to BmV, and the difference [AB] obtained by subtracting B from A is 30 to 110 (i.e., +30 to +110).

[0235] When the difference [AB] is 30 or more, the quality degradation caused by the decrease in ink jetting accuracy is further suppressed. From the viewpoint of this effect, the difference [AB] is more preferably 40 or more, and even more preferably 45 or more.

[0236] When the difference [AB] is 110 or less, the quality degradation caused by ink injection timing deviation is further suppressed. From the viewpoint of this effect, the difference [AB] is more preferably 90 or less, and more preferably 70 or less.

[0237] From the viewpoint of further suppressing image quality degradation, the ink application process is preferably carried out under the condition that the difference [AB] is 45 to 70, and the ink is applied to the non-permeable substrate.

[0238] The zeta potential (“B” (in mV) of the ink is preferably -80mV to -10mV, more preferably -80mV to -20mV, and even more preferably -80mV to -30mV.

[0239] When the zeta potential of the ink is above -80mV, it is easier to achieve a difference [AB] of less than 110.

[0240] When the zeta potential of the ink is below -20mV, it is easier to achieve a difference [AB] of 30 or more.

[0241] The zeta potential of ink can be adjusted by changing the types of ingredients contained in the ink and the composition of the ink.

[0242] The zeta potential of ink can be adjusted, for example, by adjusting the acid value and / or neutralization degree of the pigment dispersant contained in the ink as needed, the acid value and / or neutralization degree of the resin particles contained in the ink as needed, and the acid value and / or neutralization degree of the water-soluble resin contained in the ink as needed.

[0243] In this invention, the Zeta potential of the ink is represented by a value obtained by measurement using a ZETASIZER NANO-ZS manufactured by Malvern.

[0244] Specifically, the Zeta potential of the ink in this invention is determined by diluting the ink 1000 times with ultrapure water, oscillating it for 30 seconds, and then measuring it using a ZETASIZER NANO-ZS.

[0245] The electrostatic charge (“A” (in kV) of the ink-coated surface of the non-permeable substrate is preferably 0kV to 50kV (i.e., 0kV to +50kV), more preferably 5kV to 40kV, and even more preferably 10kV to 30kV.

[0246] When the electrostatic charge on the surface of the non-permeable substrate to which the ink is applied is 0 kV or higher, it is easier to achieve a difference [AB] of 30 or higher.

[0247] When the electrostatic charge on the surface of the non-permeable substrate to which the ink is applied is 50kV or less, it is easier to achieve a difference [AB] of 110 or less.

[0248] In this invention, the electrostatic charge of the ink-coated surface of a non-permeable substrate is expressed as a value obtained by measuring using an electrostatic meter SK-H050 manufactured by KEYENCECORPORATION.

[0249] Specifically, using the electrostatic measuring instrument described above, in Far (wide range mode), the charged potential is measured at a position 10 cm away from the ink-coated surface of the non-permeable substrate, and the obtained charged potential is set as the electrostatic quantity of the ink-coated surface of the non-permeable substrate.

[0250] The amount of static electricity on the ink-coated surface of a non-permeable substrate can be adjusted, for example, by using an ion generator, an antistatic brush, or an antistatic sheet.

[0251] (Heating and drying of ink)

[0252] In the ink application process, ink can be applied to a non-permeable substrate by heating and drying.

[0253] Examples of mechanisms for heating and drying include known heating mechanisms such as infrared heaters, known air supply mechanisms such as dryers, and mechanisms combining two or more of these mechanisms.

[0254] Examples of methods for heat drying include:

[0255] A method of blowing warm or hot air onto the ink-coated surface of a non-permeable substrate;

[0256] Methods of heating an ink-coated surface of a non-permeable substrate from the side with the ink and / or the side opposite to the ink-coated surface using an infrared heater, etc.; and

[0257] Combining multiple methods from these, etc.

[0258] The heating temperature during heating and drying is preferably 55°C or higher, more preferably 60°C or higher, and especially preferably 65°C or higher. There is no particular upper limit to the heating temperature; for example, 100°C could be considered, but 90°C is preferred.

[0259] There is no particular limitation on the heating and drying time, but it is preferred to be 3 to 60 seconds, more preferably 5 to 30 seconds, and especially preferably 5 to 20 seconds.

[0260] <Method of using ink sets>

[0261] In the recording method of the present invention, two or more ink groups containing water can be used.

[0262] For example, in the recording method of the present invention, an ink group comprising at least one coloring ink (hereinafter also simply referred to as "coloring ink") containing water and coloring pigment and at least one white ink (hereinafter also simply referred to as "white ink") containing water and white pigment can be used.

[0263] The ink set containing colored ink and white ink may further contain the aforementioned pretreatment solution.

[0264] In the recording method of the present invention, when using an ink group including colored ink and white ink, in the ink application process, under the conditions of the following conditions a1, a2 and a3, the colored ink and white ink are respectively applied to the same surface of the non-permeable substrate by inkjet printing.

[0265] Condition a1…The polarity of the Zeta potential of all inks, including at least one colored ink and at least one white ink, is the same.

[0266] Condition a2… The electrostatic polarity of the same side of the aforementioned non-permeable substrate is opposite to the polarity of the zeta potential of all the aforementioned inks.

[0267] Condition a3... When the electrostatic charge of the same side of the above-mentioned non-permeable substrate is set to AkV, and the Zeta potential of each of the above-mentioned at least one colored ink and the above-mentioned at least one white ink is set to BmV, for all the above-mentioned inks, the value obtained by subtracting B from A, i.e., the difference [AB], is 30 to 110.

[0268] In the recording method of the present invention, when using an ink group comprising colored ink and white ink, an image derived from these inks can be obtained. At this time, for each of these inks, a decrease in jetting accuracy and jetting timing deviation are suppressed. As a result, in the obtained image, quality degradation (e.g., the generation of streaks) caused by a decrease in jetting accuracy and / or jetting timing deviation is suppressed.

[0269] In the recording method of the present invention, it is preferable that when using an ink group including colored ink and white ink, the difference [AB] between the colored ink and the white ink is the largest among the differences [AB] between the two inks.

[0270] Therefore, the quality degradation (e.g., the formation of streaks) caused by the decrease in ink jetting accuracy and / or jetting timing deviation is more effectively suppressed in the obtained image.

[0271] The reason for this effect is believed to be that the final ink injection precision and injection timing have the greatest impact on the quality of the obtained image.

[0272] In the recording method of the present invention, when using an ink group including colored ink and white ink, if two or more integers are set to n, the difference [AB] of the ink given in the nth order is the same as or greater than the difference [AB] of the ink given in the (n-1)th order, and the difference [AB] of the last ink given is greater than the difference [AB] of the first ink given.

[0273] Therefore, the quality degradation (e.g., the formation of streaks) caused by the decrease in ink jetting accuracy and / or jetting timing deviation is more effectively suppressed in the obtained image.

[0274] The reason for this effect is believed to be that the influence of ink on the quality of the obtained image increases as the order in which ink is applied increases.

[0275] In the recording method of the present invention, when using an ink group comprising colored ink and white ink, the colored ink and white ink are applied sequentially in the ink application step, for example. That is, the white ink is applied last.

[0276] In this embodiment, for example, a transparent substrate is used as the non-permeable substrate. A colored image (i.e., a color image or a black and white image; for example, a pattern image such as text or graphics) based on colored ink is recorded on the non-permeable substrate. A white image (e.g., a solid image) based on white ink is recorded on the non-permeable substrate where the colored image is recorded to cover the colored image. In this case, when viewed from the non-image recording side (i.e., the side where no image is recorded) of the non-permeable substrate, the colored image with the white image as a background can be identified through the non-permeable substrate. On the other hand, when viewed from the image recording side (i.e., the side where the image is recorded) of the non-permeable substrate, the colored image and the non-permeable substrate are hidden by the white image based on white ink, making it difficult to identify the colored image and the non-permeable substrate.

[0277] <Pretreatment solution application process>

[0278] The recording method of the present invention may further include a pretreatment liquid application step of applying a pretreatment liquid containing water and a coagulant to a non-permeable substrate before the ink application step.

[0279] In this case, during the ink application process, ink is applied to the area on the non-permeable substrate that has been treated with the pretreatment solution.

[0280] According to this method, by using a coagulant to coagulate the components in the ink, a higher quality image can be obtained.

[0281] In the case where the recording method of the present invention includes a pretreatment liquid application step, the static electricity and static electricity amount of the "ink-applied surface of the non-permeable substrate" in the ink application step represent the static electricity and static electricity amount of the area on the non-permeable substrate to which the pretreatment liquid has been applied.

[0282] (Pretreatment solution)

[0283] The pretreatment solution contains water and a coagulant.

[0284] -water-

[0285] The pretreatment solution contains water.

[0286] The water content relative to the total amount of the pretreatment solution is preferably 50% by mass or more, and more preferably 60% by mass or more.

[0287] The upper limit of water content depends on the amount of other components, but it is preferably less than 90% by mass relative to the total amount of pretreatment solution.

[0288] -Flocculant-

[0289] The pretreatment solution prepares a coagulant, which is at least one selected from the group consisting of organic acids, organic acid salts, polyvalent metal compounds and metal complexes.

[0290] A coagulant is a component that causes components (e.g., resins) in an ink to coagulate.

[0291] -Organic acids-

[0292] Organic acids can be exemplified by organic compounds that have acidic groups.

[0293] Examples of acidic groups include phosphate groups, phosphonic acid groups, hypophosphonic acid groups, sulfuric acid groups, sulfonic acid groups, sulfinic acid groups, and carboxyl groups.

[0294] From the viewpoint of ink coagulation speed, the aforementioned acidic group is preferably a phosphate group or a carboxyl group, more preferably a carboxyl group.

[0295] In addition, the acidic groups mentioned above are preferably at least partially dissociated in the pretreatment solution.

[0296] Preferred organic compounds with carboxyl groups include polyacrylic acid, acetic acid, formic acid, benzoic acid, glycolic acid, malonic acid, malic acid (preferably DL-malic acid), maleic acid, succinic acid, glutaric acid, fumaric acid, citric acid, tartaric acid, phthalic acid, adipic acid, pimelic acid, 4-methylphthalic acid, lactic acid, pyrrolidone carboxylic acid, pyranone carboxylic acid, pyrrolic carboxylic acid, furan carboxylic acid, pyridine carboxylic acid, coumaric acid, thiophenic acid, nicotinic acid, and pimelic acid. One or more of these compounds may be used.

[0297] From the viewpoint of ink coagulation speed, carboxylic acids with a valence of 2 or higher (hereinafter also referred to as polycarboxylic acids) are preferred as organic compounds with a carboxyl group.

[0298] As a polycarboxylic acid

[0299] Dicarboxylic acids or tricarboxylic acids are preferred.

[0300] More preferably, glutaric acid, malonic acid, succinic acid, adipic acid, pimelic acid, malic acid, maleic acid, fumaric acid, tartaric acid, or citric acid.

[0301] Further preferred options include glutaric acid, malonic acid, succinic acid, adipic acid, pimelic acid, malic acid, fumaric acid, tartaric acid, or citric acid.

[0302] Further optimization is made using glutaric acid, malonic acid, succinic acid, adipic acid, or pimelic acid.

[0303] Organic acids are preferably low in pKa (e.g., 1.0 to 5.0).

[0304] Therefore, by contacting organic acid compounds with lower pKa, the surface charge of pigments, polymer particles, and other particles in inks that are dispersed and stabilized by weak acidic functional groups such as carboxyl groups is reduced, thereby decreasing the dispersion stability.

[0305] The organic acid is preferably low in pKa, highly soluble in water, and has a valence of 2 or higher. More preferably, it is a divalent or trivalent acidic substance with high buffering capacity in a pH region that is lower than the pKa of the functional group (e.g., carboxyl group) that stabilizes the particle dispersion in the ink.

[0306] -organic acid salts-

[0307] As organic acid salts, examples of salts of the organic acids exemplified above can be cited.

[0308] Examples of organic acid salts include organic acid salts of alkaline earth metals from Group 2 of the periodic table (e.g., magnesium, calcium), transition metals from Group 3 of the periodic table (e.g., lanthanum), cations from Group 13 of the periodic table (e.g., aluminum), and lanthanides (e.g., neodymium).

[0309] As an organic acid salt, an organic acid salt containing an alkaline earth metal is preferred, and an organic acid salt containing calcium (e.g., calcium lactate, calcium acetate, etc.) or an organic acid salt containing magnesium (e.g., magnesium lactate, magnesium acetate, etc.) is also preferred.

[0310] -Polyvalent metal compounds-

[0311] Examples of polyvalent metal compounds include at least one salt selected from the group consisting of alkaline earth metals (e.g., magnesium, calcium) from Group 2 of the periodic table, transition metals (e.g., lanthanum) from Group 3 of the periodic table, cations (e.g., aluminum) from Group 13 of the periodic table, and lanthanides (e.g., neodymium) (but excluding organic acid salts).

[0312] As a multivalent metal compound, nitrates, chlorides, or thiocyanates are preferred.

[0313] As a polyvalent metal compound, calcium or magnesium salts of nitric acid, calcium chloride, magnesium chloride, or calcium or magnesium salts of thiocyanate are particularly preferred.

[0314] Preferably, at least a portion of the polyvalent metal compound is dissociated into polyvalent metal ions and counterions in the pretreatment solution.

[0315] -Metal complex-

[0316] As a metal complex, it is preferred to include a metal complex containing at least one metal element selected from the group consisting of zirconium, aluminum and titanium.

[0317] As a metal complex, it is preferred to include at least one metal complex with a ligand selected from the group consisting of acetate, acetylacetonate, methyl acetoacetate, ethyl acetoacetate, octylene glycolate, butoxyacetylacetonate, lactate, ammonium lactate and triethanolamine.

[0318] As metal complexes, various metal complexes are commercially available, and commercially available metal complexes can be used in this invention. Furthermore, various multidentate ligands capable of forming various organic ligands, especially metal chelating catalysts, are commercially available. Therefore, metal complexes can be prepared by combining commercially available organic ligands and metals.

[0319] There are no particular restrictions on the amount of coagulant.

[0320] From the viewpoint of ink coagulation rate, the content of coagulant relative to the total amount of pretreatment liquid is preferably 0.1% to 40% by mass, more preferably 0.1% to 30% by mass, even more preferably 1% to 20% by mass, and particularly preferably 1% to 10% by mass.

[0321] -Resin-

[0322] The pretreatment solution preferably contains at least one resin.

[0323] Examples of resins include acrylic resins, polyester resins, polyolefin resins, polyurethane resins, polyurea resins, polyamide resins, polycarbonate resins, and polystyrene resins.

[0324] The pretreatment solution preferably contains at least one type of resin particles, i.e., resin particles.

[0325] When preparing the pretreatment solution, commercially available aqueous dispersions of resin particles can be used.

[0326] Commercially available aqueous dispersions of resin particles include Pesthresin A124GP, Pesthresin A645GH, Pesthresin A615GE, Pesthresin A520 (manufactured by TAKAMAT SU OIL&FAT CO.,LTD.), Eastek 1100, Eastek 1200 (manufactured by Eastman Chemical Company), plascoat RZ570, plascoat Z687, plascoat Z565, plascoat RZ570, plascoat Z690 (manufactured by GOO CHEMICAL CO.,LTD.), Vylonal MD1200 (manufactured by TOYOBO CO.,LTD.), EM57DOC (manufactured by Daicel FineChem Ltd.), and Superflex M500 (DKS Co. Ltd.).

[0327] When the pretreatment solution contains resin particles, the content of resin particles is preferably 0.5% to 30% by mass, more preferably 1% to 20% by mass, and especially preferably 1% to 15% by mass, relative to the total amount of the pretreatment solution.

[0328] -Water-soluble organic solvents-

[0329] The pretreatment solution may contain at least one water-soluble organic solvent.

[0330] As a water-soluble organic solvent, it is possible to use known water-soluble organic solvents without particular restrictions.

[0331] As a water-soluble organic solvent, examples of substances similar to those that can be contained in inks can be cited.

[0332] When the pretreatment solution contains a water-soluble organic solvent, the content of the water-soluble organic solvent is preferably 0.5% to 30% by mass, more preferably 1% to 20% by mass, and especially preferably 1% to 15% by mass, relative to the total amount of the pretreatment solution.

[0333] -Other ingredients-

[0334] The pretreatment solution may contain other components besides those mentioned above, as needed.

[0335] Other components that can be contained in the pretreatment solution include surfactants, solid wetting agents, silica compounds (e.g., colloidal silica), inorganic salts, anti-fading agents, emulsion stabilizers, penetration enhancers, ultraviolet absorbers, preservatives, mildew inhibitors, pH adjusters, viscosity adjusters, rust inhibitors, chelating agents, and water-soluble polymers other than water-soluble cationic polymers (e.g., water-soluble polymers described in paragraphs 0026 to 0080 of Japanese Patent Application Publication No. 2013-001854).

[0336] Other components that may be contained in the pretreatment solution may also be referenced to the components that may be contained in the first ink described later.

[0337] <Other Processes>

[0338] The recording method of the present invention may also include other steps besides those described above.

[0339] As another process, for example, is the process of laminating a laminating substrate onto an image recorded on a non-porous substrate. By laminating a laminating substrate onto an image recorded on a non-porous substrate, the image can be effectively protected.

[0340] Resin substrates are preferred as the substrate for lamination.

[0341] There are no particular limitations on the resin substrate; for example, a substrate made of thermoplastic resin can be cited.

[0342] As a resin substrate, for example, a substrate in which thermoplastic resin is molded into a sheet can be cited.

[0343] The resin substrate preferably comprises polypropylene, polyethylene terephthalate, nylon, polyethylene or polyimide.

[0344] The shape of the resin substrate is not particularly limited, but sheet-like resin substrates are preferred.

[0345] The thickness of the resin substrate is preferably 10 μm to 200 μm, and more preferably 10 μm to 100 μm.

[0346] The substrate for lamination can be laminated directly on the side of the image recorder where the image is located, or it can be laminated via other layers (e.g., adhesive layers).

[0347] When a substrate for lamination is directly laminated on the side of the image recording material to which the image is disposed, lamination can be performed by known methods such as hot pressing or hot fusion.

[0348] Furthermore, the lamination of the image recording object on the side where the image is disposed via the adhesive layer to the laminate substrate can be carried out, for example, by applying an adhesive to the side of the image recording object on which the image is recorded, then placing the laminate substrate, and then bonding the image recording object and the laminate substrate together.

[0349] Furthermore, the lamination of the side of the image recorder containing the image via the adhesive layer can also be implemented by methods such as extrusion lamination (i.e., sandwich lamination).

[0350] In the above-mentioned image recording, the adhesive layer in which the image is arranged on the side of the adhesive layer is laminated via an adhesive layer preferably contains an isocyanate compound.

[0351] When the adhesive layer contains an isocyanate compound, the lamination strength can be further improved because the adhesion between the adhesive layer and the ink source layer of the image is further enhanced.

[0352] Example

[0353] The following are embodiments of the present invention, but the present invention is not limited to the following embodiments.

[0354] The pH value was obtained by measuring the pH using a pH meter (model name: WM-50EG, manufactured by DKK-TOA CORPORATION) at 25°C.

[0355] [Examples 1-10, Comparative Examples 1-3]

[0356] Examples 1-10 and Comparative Examples 1-3 are examples and comparative examples of recording cyan monochrome images.

[0357] The following is a detailed explanation.

[0358] <Preparation of Pretreatment Solution>

[0359] A pretreatment solution was prepared by mixing the components shown below.

[0360] -Composition of the pretreatment solution-

[0361] Glutaric acid (coagulant)

[0362] …6.1% by mass

[0363] Propylene glycol (solvent)

[0364] …5.0% by mass

[0365] OLFINE E1010: (Manufactured by Nissin Chemical Co., Ltd.) [Surfactant]

[0366] …0.5% by mass

[0367] Superflex M500 (DKS Co., Ltd.) [Aqueous dispersion of urethane resin particles]

[0368] …7.0% by weight

[0369] Triisopropanolamine (pH adjuster)

[0370] …0.2% by mass

[0371] • BYK024 (BYK Corporation) [Defoamer]

[0372] …0.01% by mass

[0373] Ultrapure water

[0374] …the pretreatment solution becomes a 100% by mass residue.

[0375] <Preparation of Cyan Ink>

[0376] (Synthesis of pigment dispersant P1)

[0377] Add 965 g of dipropylene glycol to a 5000 mL three-necked flask equipped with a stirrer and cooling tube, and heat to 85 °C under a nitrogen atmosphere.

[0378] The following solutions were prepared: Solution I was obtained by dissolving 640 g of benzyl methacrylate, 340 g of methacrylic acid, and 19.94 g of 2-mercaptopropionic acid in 370.28 g of dipropylene glycol; and

[0379] Solution II was obtained by dissolving 17.69 g of tert-butyl peroxide-2-ethylhexanoate (product name "PERBUTYL O", manufactured by NOF CORPORATION) in 221.17 g of dipropylene glycol.

[0380] Solution I was added dropwise to the three-necked flask over 4 hours, and solution II was added dropwise over 5 hours. After the additions were complete, the mixture was allowed to react for an additional 2 hours. 1 H-NMR confirmed the disappearance of the monomer.

[0381] The obtained reaction solution was heated to 70°C, and 248.02 g of 50% potassium hydroxide aqueous solution was added. Then, 107.48 g of dipropylene glycol and 75.52 g of pure water were added and stirred to obtain a 37% (by mass) solution of the random polymer. This random polymer was designated as pigment dispersant P1.

[0382] pass 1¹H-NMR confirmed the structural units constituting the obtained random polymer. Furthermore, the weight-average molecular weight (Mw) was determined by GPC. The obtained pigment dispersant P1 had a weight-average molecular weight (Mw) of 8400 and an acid value of 221.7 mg KOH / g.

[0383] (Preparation of low acid value cyan pigment dispersion)

[0384] A polymer aqueous solution was prepared by dissolving 150 parts by weight of pigment dispersant P1 in water to achieve a concentration of approximately 25% by weight of pigment dispersant P1. A mixture was obtained by mixing 180 parts by weight of this 25% by weight polymer aqueous solution, 90 parts by weight of cyan pigment PB15:3 (manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd.), and 171.9 parts by weight of water. A potassium hydroxide aqueous solution was added to the obtained mixture to adjust the neutralized pH to 8.7.

[0385] Next, the neutralized mixture was dispersed for 3 hours using a bead mill (bead diameter: 0.1 mmφ, zirconia beads). This yielded a cyan pigment dispersion (uncrosslinked dispersion) containing cyan pigment dispersed in pigment dispersant P1. Water was then added to this cyan pigment dispersion to prepare an uncrosslinked dispersion C1 (pigment concentration 15% by mass).

[0386] Next, to 136 parts by weight of the uncrosslinked dispersion (C1), 3.77 parts by weight of trimethylolpropane polyglycidyl ether (product name "Denacol EX-321", manufactured by Nagase ChemteX Corporation) and 41.2 parts by weight of boric acid aqueous solution (boric acid concentration: 4% by weight) were added as crosslinking agents. The mixture was reacted at 70°C for 6 hours and then cooled to 25°C. Thus, pigment dispersant P1 was crosslinked to obtain a cyan pigment dispersion (crosslinked dispersion) in which cyan pigment was dispersed by pigment dispersant P1a. Here, pigment dispersant P1a is the polymer obtained by crosslinking the uncrosslinked polymer, i.e., pigment dispersant P1, with the crosslinking agent.

[0387] Next, ion-exchanged water was added to the above crosslinked dispersion to bring the pigment concentration to 15% by mass. The resulting liquid was then ultrafiltered at a flow rate of 600 mL per minute through an ultrafiltration apparatus (cross-flow ultrafiltration (UF), manufactured by Sartorius) equipped with a polyethersulfone (PESU) membrane (micropore size: 0.1 μm). The liquid temperature was adjusted to 25°C, and ultrafiltration was performed eight times, with each ultrafiltration cycle being equal to one volume ratio of the added liquid. Ion-exchanged water was then added to the resulting liquid to bring the pigment concentration to 15% by mass. This yielded a low-acid-value cyan pigment dispersion. The pigment dispersant P1a (low-acid-value crosslinking polymer) contained in the low-acid-value cyan pigment dispersion has an acid value of 75 mg KOH / g.

[0388] (Medium acid value cyan pigment dispersion)

[0389] Except that the amounts of 3.77 parts by weight of trimethylolpropane polyglycidyl ether (product name "Denacol EX-321", manufactured by Nagase ChemteX Corporation) and 41.2 parts by weight of boric acid aqueous solution (boric acid concentration: 4% by weight) added as crosslinking agents to 136 parts by weight of the uncrosslinked dispersion (C1) were changed to 3.00 parts by weight of trimethylolpropane polyglycidyl ether and 32.8 parts by weight of boric acid aqueous solution (boric acid concentration: 4% by weight), a medium-acid-value cyan pigment dispersion was prepared in the same manner as the preparation of the low-acid-value cyan pigment dispersion described above.

[0390] The acid value of the pigment dispersant P1b (more specifically, a polymer obtained by crosslinking pigment dispersant P1 with a crosslinking agent) contained in the medium acid value cyan pigment dispersion is 105 mg KOH / g.

[0391] (High acid value cyan pigment dispersion)

[0392] Except that the amounts of 3.77 parts by weight of trimethylolpropane polyglycidyl ether (product name "Denacol EX-321", manufactured by Nagase ChemteX Corporation) and 41.2 parts by weight of boric acid aqueous solution (boric acid concentration: 4% by weight) added as crosslinking agents to 136 parts by weight of the uncrosslinked dispersion (C1) were changed to 0.94 parts by weight of trimethylolpropane polyglycidyl ether and 10.3 parts by weight of boric acid aqueous solution (boric acid concentration: 4% by weight), a high acid value cyan pigment dispersion was prepared in the same manner as the preparation of the low acid value cyan pigment dispersion described above.

[0393] The pigment dispersant P1b (more specifically, a polymer obtained by crosslinking pigment dispersant P1 with a crosslinking agent) contained in the high acid value cyan pigment dispersion has an acid value of 185 mg KOH / g.

[0394] (Preparation of Cyan Ink C1-C3)

[0395] Cyan inks C1 to C3 were prepared by mixing the components described below.

[0396] As a cyan pigment dispersion in the following composition

[0397] The above-mentioned medium-acid-value cyan pigment dispersion is used in cyan ink C1.

[0398] The aforementioned low-acid-value cyan pigment dispersion is used in cyan ink C2.

[0399] The high-acid-value cyan pigment dispersion mentioned above was used in cyan ink C3.

[0400] -Composition of Cyan Ink C1~C3-

[0401] • Cyan pigment dispersion (pigment is CI Pigment Blue 15:3)

[0402] …The content as pigment is 4.0% by mass.

[0403] Propylene glycol (water-soluble organic solvent)

[0404] …30.0% by mass

[0405] Propylene glycol monomethyl ether (water-soluble organic solvent)

[0406] …1.0% by mass

[0407] Neocryl A-1105 (Acrylic Resin Particle Dispersion) (Manufactured by DSM)

[0408] …The content of resin particles is 5.0% by mass.

[0409] •Olfine E1010 (an acetylene glycol-based surfactant manufactured by Nissin Chemical Co., Ltd.)

[0410] …1.0% by mass

[0411] • BYK3450 (a silicone-based surfactant manufactured by BYK Corporation)

[0412] …1.0% by mass

[0413] ·PVPK15 (Polyvinylpyrrolidone K15)

[0414] …0.15% by mass

[0415] ST-XS (Colloidal Silica Dispersion) (Manufactured by Nissan Chemical Corporation)

[0416] …The content of colloidal silica particles is 0.05% by mass.

[0417] ·water

[0418] …the ink as a whole becomes 100% by mass of the remaining amount.

[0419] <Preparation of Non-Opermeable Substrates>

[0420] The following three types of non-permeable substrates (hereinafter also referred to as "substrate") are prepared.

[0421] • PET substrate…Polyethylene terephthalate substrate (product name “FE2001”, manufactured by FUTAMURA CHEMICALCO.,LTD., thickness 12μm, width 100mm, length 240mm)

[0422] • OPP substrate…biaxially stretched polypropylene substrate (FOR-AQ (20μm) manufactured by FUTAMURA CHEMICAL CO.,LTD.)

[0423] • Nylon substrate… UNITIKA LTD. manufactures Emblem ON15μm.

[0424] <Preparation of Image Recording Device>

[0425] An image recording device is provided, which includes a conveying mechanism for conveying a substrate, and sequentially includes a bar coater for applying pretreatment liquid and six inkjet heads for applying ink from the upstream side (hereinafter referred to as "upstream side") in the direction of substrate conveying.

[0426] Six nozzles are arranged along the conveying direction of the substrate.

[0427] Hereinafter, the nozzles from the upstream side are sometimes referred to as the 1st nozzle, the 2nd nozzle, the 3rd nozzle, the 4th nozzle, the 5th nozzle, and the 6th nozzle.

[0428] Each printhead is a 1200 dpi / 20 inch wide piezo full line head. Here, dpi is an abbreviation for dots per inch.

[0429] Each nozzle is a linear nozzle with nozzles arranged in a direction orthogonal to the conveying direction of the substrate (i.e., the width direction of the substrate).

[0430] The aforementioned nozzles were manufactured using the Samba G3L (manufactured by FUJIFILM Dimatix, Inc.).

[0431] <Image Recording (Cyan Monochrome)>

[0432] The substrate was subjected to corona discharge using a corona treatment machine (manufactured by KASUGA DENKI, INC., TEC-4AX, a corona surface modification evaluation device) at a discharge gap of 1 mm, 100 W, and a discharge speed of 4 m / min, thereby performing surface treatment on the substrate.

[0433] The image recording apparatus described above includes the surface-treated substrate, the pretreatment liquid, and the cyan ink (any one of cyan inks C1 to C3; see Table 1 for details). The cyan ink is set to be ejected from the second printhead. A cyan ink that has been degassed by a degassing filter and heated to 30°C is used as the cyan ink.

[0434] While the substrate is moved at a constant speed of 50 m / min, the pretreatment liquid is applied to the substrate through a wire bar coater.

[0435] The pretreatment solution was given at a mass of 1.5 g / m³. 2 .

[0436] Here, the mass of the pretreatment solution is the value obtained by dividing the mass of the pretreatment solution by the area of ​​the region to which the pretreatment solution is applied.

[0437] At the point where the pretreatment solution application ends, drying of the pretreatment solution begins using a dryer 2 seconds after the application ends at that point. The drying is performed at 60°C for 3 seconds. The residual water content, measured using a Karl Fischer moisture meter, is 0.01 g / m³. 2 the following.

[0438] Next, for the surface of the substrate that had been treated with the pretreatment solution, air was sprayed through an ion generator (manufactured by KEYENCE CORPORATION, "SJ-L005M") placed 10 cm away from the surface at a pressure of 0.05 MPa and an air flow rate of 96 L / min. The amount of static electricity was adjusted by adjusting the air pressure and air flow rate.

[0439] The electrostatic charge A (in kV) of the adjusted substrate (specifically, the surface of the substrate to which the pretreatment liquid was applied) is shown in Table 1.

[0440] While the substrate, whose electrostatic charge has been adjusted, is moved at a constant speed of 50 m / min, cyan ink (any one of cyan inks C1 to C3; see Table 1 for details) is ejected from the second nozzle and applied in a solid image pattern to the surface of the substrate that has been treated with the pretreatment liquid. At this time, the ink droplet volume is set to 2.1 ng, the duty cycle is set to 100%, and the ejection frequency is set to 39.37 kHz.

[0441] Next, 2 seconds after the ink application is completed, the cyan ink applied to the substrate is dried using an infrared (IR) irradiation device (PLC-328 manufactured by Noritake Co., Ltd.) at a surface temperature of 75°C. Then, the ink is dried in warm air at 80°C for 20 seconds using a dryer to obtain a solid cyan image.

[0442] Thus, an image recorder having a substrate and a solid blue image disposed on the substrate was obtained.

[0443] <Quality Evaluation>

[0444] The following quality assessment was performed on the solid cyan images in the image recordings.

[0445] The results are shown in Table 1.

[0446] (Injection accuracy)

[0447] In the solid cyan image, stripes along the conveying direction (specifically, dark and white stripes) are identified, and the quality caused by the spraying accuracy in the direction orthogonal to the conveying direction (i.e., the direction in which the nozzles are arranged) is evaluated according to the following evaluation criteria.

[0448] -Evaluation criteria for injection accuracy-

[0449] AA: No dark stripes or white stripes were identified.

[0450] A: The total number of dark stripes and white stripes is more than 1 and less than 4.

[0451] B: The total number of dark stripes and white stripes is more than 4 but less than 8.

[0452] C: The total number of dark and white stripes is 8 or more but less than 15.

[0453] D: The total number of dark and white stripes is 15 or more.

[0454] (Injection timing)

[0455] In the solid cyan image, the deviation of the point in the transmission direction is identified as the jet timing deviation, and the quality caused by the jet timing is evaluated according to the following evaluation criteria.

[0456] -Evaluation criteria for injection timing-

[0457] A: The injection timing deviation is less than 1 point.

[0458] B: The injection timing deviation is greater than 1 point and less than 3 points.

[0459] C: The injection timing deviation is more than 3 points but less than 5 points.

[0460] D: The injection timing deviation is more than 5 points.

[0461]

[0462] As shown in Table 1, in Examples 1 to 10, where the electrostatic polarity of the ink-bearing surface of the non-permeable substrate is opposite to the polarity of the ink's zeta potential, the quality degradation caused by the decrease in ink ejection accuracy and ejection timing deviation was suppressed in the obtained images.

[0463] In contrast, under the condition that the electrostatic polarity of the surface of the non-permeable substrate to which the ink is applied is the same as the polarity of the ink's Zeta potential, in Comparative Examples 1 to 3 where ink is applied to the non-permeable substrate, a decrease in quality occurred in the obtained images due to a decrease in ink ejection accuracy and / or ejection timing deviation.

[0464] In Examples 1-10, where the ink was applied under the condition that the difference [AB] obtained by subtracting the Zeta potential B (mV) of the ink from the electrostatic charge A (kV) of the non-permeable substrate with the ink applied was 30-110, the quality degradation caused by the decrease in ink spraying accuracy was further suppressed compared to Example 4, where the difference [AB] was less than 30.

[0465] In Examples 1 and 2, in Example 2 where the difference [AB] is 45 or more, the quality decline caused by the decrease in ink jetting accuracy is further suppressed.

[0466] In Examples 3 and 5, in Example 3 where the difference [AB] is 70 or less, the quality degradation caused by ink jetting timing deviation is further suppressed.

[0467] [Examples 101-106]

[0468] Examples 101 to 106 are examples of recording white monochrome images.

[0469] The following is a detailed explanation.

[0470] <Preparation of Pretreatment Solution>

[0471] A pretreatment solution was prepared by mixing the components shown below.

[0472] -Composition of the pretreatment solution-

[0473] Glutaric acid (coagulant)

[0474] …6.1% by mass

[0475] Propylene glycol (solvent)

[0476] …5.0% by mass

[0477] OLFINE E1010: (Manufactured by Nissin Chemical Co., Ltd.) [Surfactant]

[0478] …0.5% by mass

[0479] Superflex M500 (DKS Co., Ltd.) [Aqueous dispersion of urethane resin particles]

[0480] …7.0% by weight

[0481] Ultrapure water

[0482] …the pretreatment solution becomes a 100% by mass residue.

[0483] <Preparation of White Ink>

[0484] (Synthesis of pigment dispersant (block polymer) for low acid value white pigment dispersion)

[0485] Referring to Synthesis Example 8 of Japanese Patent Application Publication No. 2015-83688, block polymer 1 was synthesized as a pigment dispersant for low-acid-value white pigment dispersions. Details are shown below.

[0486] Add to a reaction apparatus consisting of a 1L separable flask equipped with a stirrer, reflux condenser, thermometer, and nitrogen inlet pipe.

[0487] Diethylene glycol dimethyl ether (266 parts by weight; polymerization solvent)

[0488] 2-Iodo-2-cyanopropane (6.2 parts by mass; polymerization initiator compound),

[0489] Methyl methacrylate (MMA) (120 parts by weight; monomer),

[0490] Acrylic acid (AA) (28.8 parts by weight; monomer),

[0491] Cyclohexyl methacrylate (CHMA) (67.2 parts by weight; monomer),

[0492] Azodimethylisovalerate (7.9 parts by weight) and

[0493] 2-tert-butyl-4,6-dimethylphenol (0.7 parts by weight; catalyst),

[0494] Nitrogen gas was passed through while the mixture was stirred.

[0495] Next, the temperature of the mixture in the reaction apparatus (reaction temperature) was raised to 70°C and polymerization was carried out for 3 hours, thereby obtaining a polymerization solution A containing MMA / AA / CHMA copolymer.

[0496] Three hours later, a portion of the above-mentioned polymerization solution A was sampled, and the result of solid content determination was 42.0% by mass, confirming that most of the monomers had polymerized.

[0497] Furthermore, the molecular weight of the MMA / AA / CHMA copolymer, as determined by GPC, was 7,500 by weight-average molecular weight (Mn).

[0498] The acid value of this MMA / AA / CHMA copolymer is 101.0 mg KOH / g.

[0499] Next, a mixture of benzyl methacrylate (BzMA) (35.2 parts by mass; monomer) and V-65 (0.3 parts by mass; free radical generator) was added to the above polymerization solution A, and polymerization was carried out at 70°C for 3 hours to obtain a polymerization solution B containing block polymer 1 as a pigment dispersant for a low acid value white pigment dispersion.

[0500] Here, block polymer 1 is a block polymer containing MMA / AA / CHMA copolymer, i.e., block A, and BzMA homopolymer, i.e. block B.

[0501] The solid content of the obtained polymerization solution B was determined to be 43.2% by mass, confirming that most of the monomers had polymerized.

[0502] Furthermore, the block polymer 1 has a Mw of 8,500 and an acid value of 89.3 mg KOH / g.

[0503] (Preparation of low acid value white pigment dispersion)

[0504] The block polymer 1 (136.4 parts by mass), butylcarbitol (163.6 parts by mass), and CI Pigment White 6 (trade name "JR-405", titanium dioxide particles, manufactured by TAYCA Co., Ltd.) (450 parts by mass) as a white pigment were blended and stirred using a disperser. Next, the white pigment was thoroughly dispersed using a horizontal media disperser to obtain an oily pigment dispersion. The average particle size of the white pigment dispersed in the oily pigment dispersion was 290 nm. The viscosity of the oily pigment dispersion was 86.3 mPa·s.

[0505] Next, while stirring the above-mentioned oily pigment dispersion (700 parts by weight) using a disperser, a mixture of potassium hydroxide (4.0 parts by weight) and water (341 parts by weight) was slowly added to neutralize it. Then, the white pigment was fully dispersed using a horizontal media disperser to obtain a pigment dispersion.

[0506] Next, the obtained pigment dispersion was ultrafiltered using an ultrafiltration apparatus (cross-flow ultrafiltration (UF), manufactured by Sartorius) with ion-exchanged water flowing through it at a flow rate of 600 mL per minute. The liquid temperature was maintained at 25°C, and ultrafiltration was performed 10 times, with each cycle consisting of one volume of liquid added. Ion-exchanged water was then added, resulting in a low-acid-value white pigment dispersion with a white pigment concentration of 45% by mass and a block polymer concentration of 3.7% by mass.

[0507] (Preparation of a medium-acid-value white pigment dispersion)

[0508] -Synthesis of Pigment Dispersant P1-

[0509] Pigment dispersant P1 (uncrosslinked polymer) was synthesized, which is the same pigment dispersant P1 used in the preparation of the above-mentioned cyan pigment dispersions.

[0510] Preparation of a white pigment separation solution with medium acid value -

[0511] Pigment dispersant P1 (150 parts by mass) was dissolved in water to prepare a polymer solution with a concentration of 25% by mass of pigment dispersant P1.

[0512] A mixture was obtained by mixing 96 parts by mass of the above polymer solution, 300 parts by mass of white pigment CI Pigment White 6 (trade name "JR-405", titanium dioxide particles, manufactured by TAYCA Co., Ltd.), and 270 parts by mass of water. A potassium hydroxide aqueous solution was added to the obtained mixture to adjust the pH to 8.7 after neutralization.

[0513] Next, the neutralized mixture was dispersed for 3 hours using a bead mill (bead diameter: 0.1 mmφ, zirconia beads). This yielded a white pigment dispersion (uncrosslinked dispersion) PD1, in which white pigment was dispersed by pigment dispersant P1.

[0514] Next, the obtained white pigment dispersion (uncrosslinked dispersion) PD1 was ultrafiltered using an ultrafiltration apparatus (cross-flow ultrafiltration (UF), manufactured by Sartorius) with ion-exchanged water flowing through it at a flow rate of 600 mL per minute. The liquid temperature was maintained at 25°C, and ultrafiltration was performed three times, with each ultrafiltration cycle consisting of one volume of liquid added. Ion-exchanged water was then added to the ultrafiltered liquid to obtain an ultrafiltered dispersion with a white pigment concentration of 45% by mass and a pigment dispersant concentration of 3.6% by mass P1.

[0515] To 136 parts by weight of the ultrafiltration dispersion described above, 1.35 parts by weight of trimethylolpropane polyglycidyl ether (product name "Denacol EX-321", manufactured by Nagase ChemteX Corporation) as a crosslinking agent and 14.5 parts by weight of boric acid aqueous solution (boric acid concentration: 4% by weight) were added. After reacting at 70°C for 6 hours, the mixture was cooled to 25°C. Thus, the pigment dispersant P1 in the crosslinked dispersion formed a crosslinked polymer dispersant, i.e., pigment dispersant P1a, thereby obtaining a white pigment dispersion (crosslinked dispersion) in which white pigment is dispersed by the crosslinked polymer dispersant L1, i.e., pigment dispersant P1a.

[0516] Ion-exchanged water was added to the obtained crosslinked dispersion to bring the pigment concentration to 15% by mass. The crosslinked dispersion with added ion-exchanged water was then passed at a flow rate of 600 mL per minute through an ultrafiltration apparatus (cross-flow ultrafiltration unit (UF), manufactured by Sartorius) equipped with a polyethersulfone (PESU) membrane (micropore size: 0.1 μm). The liquid temperature was adjusted to 25°C, and ultrafiltration was performed three times, with each pass being equal to one volume ratio of the added liquid. Next, ion-exchanged water was added to bring the white pigment concentration to 45% by mass. This yielded a white pigment dispersion with a medium acid value.

[0517] The acid value of pigment dispersant P1a contained in the medium-acid-value white pigment dispersion is 144 mg KOH / g. Furthermore, the concentration of pigment dispersant P1a is 3.6% by mass.

[0518] Pigment dispersant P1a is an uncrosslinked polymer, that is, pigment dispersant P1 is a crosslinked polymer formed by crosslinking polyethylene glycol diglycidyl ether as a crosslinking agent.

[0519] (Preparation of high acid value white pigment dispersion)

[0520] Except that the amounts of 1.35 parts by weight of trimethylolpropane polyglycidyl ether (product name "Denacol EX-321", manufactured by Nagase ChemteX Corporation) and 14.5 parts by weight of boric acid aqueous solution (boric acid concentration: 4% by weight) added as crosslinking agents to 136 parts by weight of the ultrafiltration dispersion were changed to 0.63 parts by weight of trimethylolpropane polyglycidyl ether and 7.25 parts by weight of boric acid aqueous solution (boric acid concentration: 4% by weight), a high acid value white pigment dispersion was prepared in the same manner as the preparation of the medium acid value white pigment dispersion described above.

[0521] The pigment dispersant P1b (more specifically, a polymer obtained by crosslinking pigment dispersant P1 with a crosslinking agent) contained in the high acid value white pigment dispersion has an acid value of 185 mg KOH / g.

[0522] (Preparation of white inks W1 to W3)

[0523] White inks W1 to W3 were prepared by mixing the components described below.

[0524] As a white pigment dispersion in the following composition

[0525] The above-mentioned medium-acid-value white pigment dispersion is used in white ink W1.

[0526] The aforementioned low-acid-value white pigment dispersion was used in white ink W2.

[0527] The aforementioned high-acid-value white pigment dispersion was used in white ink W3.

[0528] -Composition of white inks W1 to W3-

[0529] White pigment dispersion

[0530] …14% by mass (as pigment content)

[0531] Propylene glycol (water-soluble organic solvent)

[0532] …30% by mass

[0533] Propylene glycol monomethyl ether (water-soluble organic solvent)

[0534] …1% by mass

[0535] Neocryl A-1105 (Acrylic polymer resin particle dispersion) (manufactured by DSM Corporation)

[0536] …5.0% by mass (as content of resin particles)

[0537] •Olfine E1010 (an acetylene glycol-based surfactant manufactured by Nissin Chemical Co., Ltd.)

[0538] …1.0% by mass

[0539] • BYK3450 (a silicone-based surfactant manufactured by BYK Corporation)

[0540] …1.0% by mass

[0541] ·PVPK15 (Polyvinylpyrrolidone K15)

[0542] …0.15% by mass

[0543] ST-XS (Colloidal Silica Dispersion) (Manufactured by Nissan Chemical Corporation)

[0544] …The content of colloidal silica particles is 0.05% by mass.

[0545] ·water

[0546] …totaling to a surplus of 100% by mass

[0547] <Preparation of Substrate and Image Recording Device>

[0548] The same substrate (i.e., non-permeable substrate) and image recording device as those used in Example 1 were prepared.

[0549] <Image Recording (White Monochrome)>

[0550] In addition to replacing the cyan ink set to be ejected from the second printhead, white ink (any one of white inks W1 to W3, see Table 2 for details) was used, set to be ejected from the fifth printhead, and the ink droplet volume was changed to 4.0 ng. The same operation as the image recording in Example 1 was performed, thereby obtaining an image record having a substrate and a white solid image provided on the substrate.

[0551] <Quality Evaluation>

[0552] The same quality evaluation was performed on the white solid image in the image record as on the cyan solid image in Example 1.

[0553] The results are shown in Table 2.

[0554] [Table 2]

[0555]

[0556] As shown in Table 2, in Examples 101 to 106, under the same conditions as Examples 1 to 10, where the electrostatic polarity of the ink-bearing surface of the non-permeable substrate is opposite to the polarity of the ink's zeta potential, the quality degradation caused by the decrease in ink ejection accuracy and ejection timing deviation was suppressed in the obtained images when ink was applied to the non-permeable substrate.

[0557] [Examples 201-209]

[0558] Examples 201-209 are examples of recording multi-layered images using an ink set comprising a pretreatment liquid, a coloring ink (specifically, at least one of black ink, cyan ink, magenta ink, and yellow ink), and a white ink. The details are described below.

[0559] <Preparation of Pretreatment Solution>

[0560] The same pretreatment solution as that prepared in Example 101 was prepared.

[0561] <Preparation of Cyan Ink>

[0562] The aforementioned cyan inks C1 and C2 were prepared.

[0563] <Preparation of White Ink>

[0564] The aforementioned white ink W1 was prepared.

[0565] <Preparation of Black Ink>

[0566] (Synthesis of pigment dispersant P1)

[0567] Pigment dispersant P1 (uncrosslinked polymer) was synthesized, which is the same pigment dispersant P1 used in the preparation of the above-mentioned cyan pigment dispersions.

[0568] (Preparation of black pigment dispersion)

[0569] A polymer aqueous solution was prepared by dissolving 150 parts by weight of pigment dispersant P1 in water to achieve a concentration of approximately 25% by weight of pigment dispersant P1. A mixture was obtained by mixing 180 parts by weight of this 25% by weight polymer aqueous solution, 110.0 parts by weight of carbon black pigment FW182 (manufactured by Orion), and 240.0 parts by weight of water. A potassium hydroxide aqueous solution was added to the obtained mixture to adjust the neutralized pH to 8.7.

[0570] Next, the neutralized mixture was dispersed for 3 hours using a bead mill (bead diameter: 0.1 mm φ, zirconia beads). This yielded a black pigment dispersion (uncrosslinked dispersion) containing black pigment dispersed in pigment dispersant P1. Water was then added to the black pigment dispersion to prepare an uncrosslinked dispersion K1 (pigment concentration 15% by mass).

[0571] Next, 2.40 parts by mass of trimethylolpropane polyglycidyl ether (product name "Denacol EX-321", manufactured by Nagase ChemteX Corporation) and 26.2 parts by mass of boric acid aqueous solution (boric acid concentration: 4% by mass) as crosslinking agents were added to 136 parts by mass of the uncrosslinked dispersion (K1). After reacting at 70°C for 6 hours, the mixture was cooled to 25°C. Thus, pigment dispersant P1 was crosslinked to obtain a black pigment dispersion (crosslinked dispersion) in which black pigment was dispersed by pigment dispersant P1a. Here, pigment dispersant P1a is a polymer obtained by crosslinking the uncrosslinked polymer, i.e., pigment dispersant P1, with a crosslinking agent.

[0572] Next, ion-exchanged water was added to the above crosslinked dispersion to bring the pigment concentration to 15% by mass. The resulting liquid was then ultrafiltered at a flow rate of 600 mL per minute through an ultrafiltration apparatus (cross-flow ultrafiltration (UF), manufactured by Sartorius) equipped with a polyethersulfone (PESU) membrane (micropore size: 0.1 μm). The liquid temperature was adjusted to 25°C, and ultrafiltration was performed eight times, with each ultrafiltration cycle being equal to one volume ratio of the added liquid. Ion-exchanged water was then added to the resulting liquid to bring the pigment concentration to 15% by mass. This yielded a black pigment dispersion. The pigment dispersant P1a (crosslinked polymer) contained in the black pigment dispersion had an acid value of 105 mg KOH / g.

[0573] (Preparation of black ink K1)

[0574] Black ink K1 was prepared by mixing the components described below.

[0575] -Composition of black ink K1-

[0576] The above-mentioned black pigment dispersion

[0577] …The content as pigment is 5.0% by mass.

[0578] Propylene glycol (water-soluble organic solvent)

[0579] …30.0% by mass

[0580] Propylene glycol monomethyl ether (water-soluble organic solvent)

[0581] …1.0% by mass

[0582] Neocryl A-1105 (Acrylic polymer resin particle dispersion) (manufactured by DSM Corporation)

[0583] …The content of resin particles is 5.0% by mass.

[0584] •Olfine E1010 (an acetylene glycol-based surfactant manufactured by Nissin Chemical Co., Ltd.)

[0585] …1.0% by mass

[0586] • BYK3450 (a silicone-based surfactant manufactured by BYK Corporation)

[0587] …1.0% by mass

[0588] ·PVPK15 (Polyvinylpyrrolidone K15)

[0589] …0.15% by mass

[0590] ST-XS (Colloidal Silica Dispersion) (Manufactured by Nissan Chemical Corporation)

[0591] …The content of colloidal silica particles is 0.05% by mass.

[0592] ·water

[0593] …totaling to a remaining amount of 100% by mass

[0594] <Preparation of Magenta Ink>

[0595] (Preparation of PR-122 dispersion)

[0596] The operation of "mixing 180 parts by mass of 25% polymer aqueous solution, 110.0 parts by mass of carbon black pigment FW182 (manufactured by Orion), and 240.0 parts by mass of water" has been changed to

[0597] The mixture consisted of 180 parts by weight of a 25% by weight polymer aqueous solution and a magenta pigment, PR-122.

[0598] The operation involves mixing 90 parts by weight of Pigment Red 122 (FUJI Fast Red (registered trademark), manufactured by Fuji Pigment Co., Ltd.) and 171.9 parts by weight of water, and...

[0599] The operation of "adding 2.40 parts by weight of trimethylolpropane polyglycidyl ether (product name "Denacol EX-321", manufactured by Nagase ChemteX Corporation) and 26.2 parts by weight of boric acid aqueous solution (boric acid concentration: 4% by weight) as a crosslinking agent" will be changed to

[0600] In addition to the operation of "adding 3.00 parts by weight of trimethylolpropane polyglycidyl ether (product name "Denacol EX-321", manufactured by Nagase ChemteX Corporation as a crosslinking agent and 32.8 parts by weight of boric acid aqueous solution (boric acid concentration: 4% by weight)",

[0601] PR-122 dispersion was prepared in the same manner as the preparation of the black pigment dispersion described above.

[0602] The pigment dispersant P1a (crosslinked polymer) contained in the PR-122 dispersion has an acid value of 105 mg KOH / g.

[0603] (Preparation of PR-254 Dispersion A)

[0604] Except for replacing PR-122 with the same amount of PR-254 (CI Pigment Red 254), PR-254 dispersion A was obtained in the same manner as the preparation of PR-122 dispersion.

[0605] The pigment dispersant P1a (crosslinked polymer) contained in PR-254 dispersion A has an acid value of 105 mg KOH / g.

[0606] (Preparation of PR-150 dispersion)

[0607] Except for replacing PR-122 with the same amount of PR-150 (CI Pigment Red 150), a PR-150 dispersion was obtained in the same manner as the preparation of the PR-122 dispersion.

[0608] The pigment dispersant P1a (crosslinked polymer) contained in the PR-150 dispersion has an acid value of 105 mg KOH / g.

[0609] (Preparation of PR-254 Dispersion B)

[0610] Except that the amounts of 3.00 parts by weight of trimethylolpropane polyglycidyl ether (product name "Denacol EX-321", manufactured by Nagase ChemteX Corporation) and 32.8 parts by weight of boric acid aqueous solution (boric acid concentration: 4% by weight) added as crosslinking agents to 136 parts by weight of the uncrosslinked dispersion were changed to 0.94 parts by weight of trimethylolpropane polyglycidyl ether and 10.3 parts by weight of boric acid aqueous solution (boric acid concentration: 4% by weight), PR-254 dispersion B was prepared in the same manner as the preparation of PR-254 dispersion A described above.

[0611] The pigment dispersant P1b contained in PR-254 dispersion B (more specifically, a polymer obtained by crosslinking pigment dispersant P1 with a crosslinking agent) has an acid value of 185 mg KOH / g.

[0612] (Preparation of magenta ink M1)

[0613] Magenta ink M1 was prepared by mixing the components described below.

[0614] -Composition of magenta ink M1-

[0615] The above PR-122 dispersion

[0616] …The content as pigment is 4.5% by mass.

[0617] • The above PR-254 dispersion A

[0618] …The content as pigment is 1.5% by mass.

[0619] Propylene glycol (water-soluble organic solvent)

[0620] …30.0% by mass

[0621] Propylene glycol monomethyl ether (water-soluble organic solvent)

[0622] …1.0% by mass

[0623] Neocryl A-1105 (Acrylic polymer resin particle dispersion) (manufactured by DSM Corporation)

[0624] …The content of resin particles is 5.0% by mass.

[0625] •Olfine E1010 (an acetylene glycol-based surfactant manufactured by Nissin Chemical Co., Ltd.)

[0626] …1.0% by mass

[0627] • BYK3450 (a silicone-based surfactant manufactured by BYK Corporation)

[0628] …1.0% by mass

[0629] ·PVPK15 (Polyvinylpyrrolidone K15)

[0630] …0.15% by mass

[0631] ST-XS (Colloidal Silica Dispersion) (Manufactured by Nissan Chemical Corporation)

[0632] …The content of colloidal silica particles is 0.05% by mass.

[0633] ·water

[0634] …totaling to a remaining amount of 100% by mass

[0635] (Preparation of magenta ink M2)

[0636] Magenta ink M2 was prepared by mixing the components described below.

[0637] -Composition of magenta ink M2-

[0638] The above PR-122 dispersion

[0639] …The content as pigment is 4.5% by mass.

[0640] • The above PR-254 dispersion B

[0641] …The content as pigment is 1.5% by mass.

[0642] Propylene glycol (water-soluble organic solvent)

[0643] …30.0% by mass

[0644] Propylene glycol monomethyl ether (water-soluble organic solvent)

[0645] …1.0% by mass

[0646] Neocryl A-1105 (Acrylic polymer resin particle dispersion) (manufactured by DSM Corporation)

[0647] …The content of resin particles is 5.0% by mass.

[0648] •Olfine E1010 (an acetylene glycol-based surfactant manufactured by Nissin Chemical Co., Ltd.)

[0649] …1.0% by mass

[0650] • BYK3450 (a silicone-based surfactant manufactured by BYK Corporation)

[0651] …1.0% by mass

[0652] ·PVPK15 (Polyvinylpyrrolidone K15)

[0653] …0.15% by mass

[0654] ST-XS (Colloidal Silica Dispersion) (Manufactured by Nissan Chemical Corporation)

[0655] …The content of colloidal silica particles is 0.05% by mass.

[0656] ·water

[0657] …totaling to a remaining amount of 100% by mass

[0658] (Preparation of magenta ink M3)

[0659] Magenta ink M3 was prepared by mixing the components described below.

[0660] -Composition of magenta ink M3-

[0661] The above PR-122 dispersion

[0662] …The content as pigment is 4.5% by mass.

[0663] • The above PR-150 dispersion

[0664] …The content as pigment is 1.5% by mass.

[0665] Propylene glycol (water-soluble organic solvent)

[0666] …30.0% by mass

[0667] Propylene glycol monomethyl ether (water-soluble organic solvent)

[0668] …1.0% by mass

[0669] Neocryl A-1105 (Acrylic polymer resin particle dispersion) (manufactured by DSM Corporation)

[0670] …The content of resin particles is 5.0% by mass.

[0671] •Olfine E1010 (an acetylene glycol-based surfactant manufactured by Nissin Chemical Co., Ltd.)

[0672] …1.0% by mass

[0673] • BYK3450 (a silicone-based surfactant manufactured by BYK Corporation)

[0674] …1.0% by mass

[0675] ·PVPK15 (Polyvinylpyrrolidone K15)

[0676] …0.15% by mass

[0677] ST-XS (Colloidal Silica Dispersion) (Manufactured by Nissan Chemical Corporation)

[0678] …The content of colloidal silica particles is 0.05% by mass.

[0679] ·water

[0680] …totaling to a remaining amount of 100% by mass

[0681] <Preparation of Yellow Ink>

[0682] (Preparation of yellow pigment dispersion)

[0683] The operation of "mixing 180 parts by mass of 25% polymer aqueous solution, 110.0 parts by mass of carbon black pigment FW182 (manufactured by Orion), and 240.0 parts by mass of water" has been changed to

[0684] The operation involves mixing 180 parts by weight of a 25% polymer aqueous solution, 75 parts by weight of yellow pigment PY-74 (CI Pigment Yellow 74) (manufactured by FUJI Fast Red (registered trademark), Fuji Pigment Co., Ltd.), and 140 parts by weight of water.

[0685] The operation of "adding 2.40 parts by weight of trimethylolpropane polyglycidyl ether (product name "Denacol EX-321", manufactured by Nagase ChemteX Corporation) and 26.2 parts by weight of boric acid aqueous solution (boric acid concentration: 4% by weight) as a crosslinking agent" will be changed to

[0686] In addition to the operation of "adding 3.60 parts by weight of trimethylolpropane polyglycidyl ether (product name "Denacol EX-321", manufactured by Nagase ChemteX Corporation) and 39.4 parts by weight of boric acid aqueous solution (boric acid concentration: 4% by weight) as a crosslinking agent",

[0687] A yellow pigment dispersion was prepared in the same manner as the preparation of the black pigment dispersion described above.

[0688] The pigment dispersant P1a (crosslinked polymer) contained in the yellow pigment dispersion has an acid value of 105 mg KOH / g.

[0689] (Preparation of yellow ink Y1)

[0690] Yellow ink Y1 was prepared by mixing the components described below.

[0691] -Composition of Yellow Ink Y1-

[0692] The above-mentioned yellow pigment dispersion

[0693] …The content as pigment is 4.0% by mass.

[0694] • The above PR-150 dispersion

[0695] …The content as pigment is 1.5% by mass.

[0696] Propylene glycol (water-soluble organic solvent)

[0697] …30.0% by mass

[0698] Propylene glycol monomethyl ether (water-soluble organic solvent)

[0699] …1.0% by mass

[0700] Neocryl A-1105 (Acrylic Resin Particle Dispersion) (Manufactured by DSM)

[0701] …The content of resin particles is 5.0% by mass.

[0702] •Olfine E1010 (an acetylene glycol-based surfactant manufactured by Nissin Chemical Co., Ltd.)

[0703] …1.0% by mass

[0704] • BYK3450 (a silicone-based surfactant manufactured by BYK Corporation)

[0705] …1.0% by mass

[0706] ·PVPK15 (Polyvinylpyrrolidone K15)

[0707] …0.15% by mass

[0708] ST-XS (Colloidal Silica Dispersion) (Manufactured by Nissan Chemical Corporation)

[0709] …The content of colloidal silica particles is 0.05% by mass.

[0710] ·water

[0711] …totaling to a remaining amount of 100% by mass

[0712] <Preparation of Substrate and Image Recording Device>

[0713] The same substrate (i.e., non-permeable substrate) and image recording device as those used in Example 1 were prepared.

[0714] <Image Recording (Multi-Layer Image)>

[0715] Except for the following aspects, image recording (multi-layer image) was performed in the same manner as image recording (cyan monochrome) in Example 1.

[0716] -Differences from image recording (cyan monochrome) in Example 1-

[0717] Set each ink to spray the inks shown in Table 3 from printhead 1 to printhead 6. A "-" in the Ink No. column of Table 3 indicates that the corresponding ink is not being used.

[0718] The operation on the substrate surface where the pretreatment solution was applied, after the electrostatic adjustment of applying cyan ink in a solid image pattern, is changed to...

[0719] The process involves sequentially applying the inks shown in Table 3 in a solid image pattern to the substrate surface that has been treated with the pretreatment liquid after the electrostatic amount has been adjusted.

[0720] For the ink application amount, 4.0 ng was set for white ink and 2.1 ng for other inks. The duty cycle for each ink application is shown in Table 3. All inks were applied to the same area to ensure overlap.

[0721] Next, 2 seconds after the last ink application is completed, the outermost layer of ink (i.e., the last ink applied) of all inks repeatedly applied to the substrate is dried using an infrared (IR) irradiation device (PLC-328 manufactured by Noritake Co., Ltd.) at a surface temperature of 75°C. Then, it is dried in warm air at 80°C for 20 seconds using a dryer, thereby obtaining a multi-layered solid image.

[0722] Thus, an image recorder having a substrate and multiple layers of solid images disposed on the substrate is obtained. In any embodiment, the outermost layer of the multiple layers of solid images is also a white image derived from white ink W1.

[0723] <Quality Evaluation>

[0724] The image recorder is placed on the black portion of the opacity test paper (JIS qualified) manufactured by TP Giken Co., Ltd. with the image recording surface (i.e., the surface of the substrate) in contact with the black portion.

[0725] In this state, by visually observing the multi-layered image of the image recorder from above the outermost layer, i.e., the white image, stripes (specifically, dark stripes and white stripes) can be identified.

[0726] Based on the confirmed results, and according to the following evaluation criteria, the quality was evaluated.

[0727] The stripes in this multi-layer image are defects caused by decreased injection accuracy and / or injection timing deviation.

[0728] -Quality Evaluation Standards-

[0729] AA: The total number of dark stripes and white stripes is more than 0 and less than 5.

[0730] A: The total number of dark stripes and white stripes is more than 5 but less than 10.

[0731] B: The total number of dark stripes and white stripes is more than 10 but less than 20.

[0732] C: The total number of dark and white stripes is more than 20 but less than 30.

[0733] D: The total number of dark and white stripes is more than 30.

[0734] The results are shown in Table 3.

[0735] [Table 3]

[0736]

[0737] As shown in Table 3, in Examples 201 to 209, which use an ink group containing at least one colored ink (i.e., at least one of black ink K1, cyan ink C1 to C2, magenta ink M1 to M3, and yellow ink Y1) and at least one white ink (i.e., white ink W1), under the conditions of a1, a2, and a3 below, the quality degradation (i.e., streaks) caused by the decrease in spraying accuracy and / or spraying timing deviation was suppressed when these inks were applied to the substrate respectively.

[0738] Condition a1… All inks, including at least one colored ink and at least one white ink, have the same polarity of their Zeta potential.

[0739] Condition a2… The electrostatic polarity of the same side of the non-permeable substrate is opposite to the polarity of the zeta potential of all inks.

[0740] Condition a3... When the electrostatic charge on the same side of the non-permeable substrate is set to AkV, and the Zeta potential of at least one colored ink and at least one white ink is set to BmV, for all inks, the difference [AB] obtained by subtracting B from A is 30 to 110.

[0741] The results from Examples 201 to 209 show that, among the differences [AB] of each ink, the ink with the largest difference [AB] at the end (Examples 201, 202, 205, 206, 208 and 209) further suppressed the quality decline.

[0742] [Examples 1A to 10A]

[0743] In Examples 1-10, the same operations as in Examples 1-10 were performed except that no pretreatment solution was applied.

[0744] As a result, the same effect as in Examples 1-10 was achieved.

[0745] [Examples 1B-10B, Examples 101B-106B, Examples 201B-209B]

[0746] In Examples 1-10, 101-106, and 201-209, the same operations as in Examples 1-10, 101-106, and 201-209 were performed, except that "6.1% by mass of glutaric acid" in the composition of the pretreatment solution was replaced with "0.6% by mass of glutaric acid, 5.0% by mass of adipic acid, and 0.5% by mass of succinic acid".

[0747] As a result, the same effects as in Examples 1-10, Examples 101-106 and Examples 201-209 were obtained.

[0748] [Examples 1C-10C, Examples 101C-106C, Examples 201C-209C]

[0749] In Examples 1-10, 101-106, and 201-209, the same operations as in Examples 1-10, 101-106, and 201-209 were performed, except that "6.1% by mass of glutaric acid" in the pretreatment solution was replaced with "0.6% by mass of glutaric acid, 5.0% by mass of adipic acid, and 0.5% by mass of succinic acid", and the acrylic resin particles in the ink were replaced with the same amount of styrene acrylic resin particles (as the resin particle dispersion, "Neocryl A-1109" manufactured by DSM was used).

[0750] As a result, the same effects as in Examples 1-10, Examples 101-106 and Examples 201-209 were obtained.

[0751] [Examples 1D-10D, Examples 101D-106D, Examples 201D-209D]

[0752] In Examples 1-10, 101-106, and 201-209, the same operations as in Examples 1-10, 101-106, and 201-209 were performed, except that “6.1% by mass of glutaric acid” in the composition of the pretreatment solution was replaced with “5.0% by mass of calcium formate and 3.0% by mass of calcium lactate”.

[0753] As a result, the same effects as in Examples 1-10, Examples 101-106 and Examples 201-209 were obtained.

[0754] [Examples 1E-10E, Examples 101E-106E, Examples 201E-209E]

[0755] In Examples 1-10, 101-106, and 201-209, the same operations as in Examples 1-10, 101-106, and 201-209 were performed, except that "6.1% by mass of glutaric acid" in the pretreatment solution was replaced with "5.0% by mass of calcium formate and 3.0% by mass of calcium lactate", and the acrylic resin in the ink was replaced with the same amount of styrene acrylic resin (Neocryl A-1109, manufactured by DSM).

[0756] As a result, the same effects as in Examples 1-10, Examples 101-106 and Examples 201-209 were obtained.

[0757] [Examples 1F-10F, Examples 101F-106F, Examples 201F-209F]

[0758] In Examples 1-10, 101-106, and 201-209, the same operations as in Examples 1-10, 101-106, and 201-209 were performed, except that "6.1% by mass of glutaric acid" in the pretreatment solution was replaced with "5.0% by mass of calcium formate and 3.0% by mass of calcium lactate", and the acrylic resin particles in the ink were replaced with the same amount of urethane resin particles (using "Superflex 460" manufactured by DKSCo.Ltd. as the resin particle dispersion).

[0759] As a result, the same effects as in Examples 1-10, Examples 101-106 and Examples 201-209 were obtained.

[0760] [Examples 1G-10G, Examples 101G-106G, Examples 201G-209G]

[0761] In Examples 1-10, 101-106, and 201-209, the same operations as in Examples 1-10, 101-106, and 201-209 were performed, except that "6.1% by mass of glutaric acid" in the composition of the pretreatment solution was replaced with "0.6% by mass of glutaric acid, 5.0% by mass of adipic acid, and 0.5% by mass of succinic acid", and the acrylic resin particles in the ink were replaced with the same amount of urethane resin particles (using "Superflex 460" manufactured by DKS Co. Ltd. as the resin particle dispersion).

[0762] As a result, the same effects as in Examples 1-10, Examples 101-106 and Examples 201-209 were obtained.

[0763] The invention of Japanese Patent Application No. 2021-191601, filed on November 25, 2021, is incorporated herein by reference in its entirety.

[0764] All documents, patent applications and technical standards described in this specification are incorporated herein by reference to the same extent as the specific documents, patent applications and technical standards which are incorporated herein by reference.

Claims

1. An inkjet recording method, comprising an ink application step, wherein an ink containing water is applied to a non-porous substrate by inkjet printing. In the ink application process, the ink is applied to the non-permeable substrate under conditions where the electrostatic polarity of the surface on which the ink is applied is opposite to the polarity of the zeta potential of the ink. In the ink application process, the ink is applied to the non-permeable substrate when the electrostatic charge of the surface on which the ink is applied is set to AkV and the Zeta potential of the ink is set to BmV, and the difference [AB] obtained by subtracting B from A is 30 to 110.

2. The inkjet recording method according to claim 1, wherein, In the ink application process, the ink is applied to the non-permeable substrate under the condition that the difference [AB] is 45 to 70.

3. The inkjet recording method according to claim 1, wherein, The zeta potential of the ink is -80mV to -30mV.

4. The inkjet recording method according to claim 1, wherein, The electrostatic charge on the surface of the non-permeable substrate to which the ink is applied is 10kV to 30kV.

5. The inkjet recording method according to claim 1, wherein, The non-permeable substrate is a resin substrate.

6. The inkjet recording method according to claim 1, further comprising a pretreatment solution application step, wherein, prior to the ink application step, a pretreatment solution containing water and a coagulant is applied to the non-permeable substrate. In the ink application process, the ink is applied to the area on the non-permeable substrate that has been treated with the pretreatment liquid.

7. The inkjet recording method according to claim 1, wherein, The ink group comprises at least one coloring ink containing water and coloring pigment, and at least one white ink containing water and white pigment. The coloring ink refers to ink of any color other than white, and the coloring pigment refers to pigment of any color other than white. In the ink application process, under the conditions a1, a2, and a3 below, the at least one colored ink and the at least one white ink are respectively applied to the same surface of the non-permeable substrate by inkjet printing. Condition a1: The polarity of the Zeta potential of all inks, including the at least one colored ink and the at least one white ink, is the same. Condition a2: The electrostatic polarity of the same side of the non-permeable substrate is opposite to the polarity of the Zeta potential of all the inks. Condition a3: When the electrostatic charge of the same side of the non-permeable substrate is set to AkV, and the Zeta potential of each of the at least one colored ink and the at least one white ink is set to BmV, for all the inks, the difference [AB] obtained by subtracting B from A is 30 to 110.

8. The inkjet recording method according to claim 7, wherein, Of the differences [AB] between the at least one colored ink and the at least one white ink, the difference [AB] of the last ink applied is the largest.

9. The inkjet recording method according to claim 7, wherein, In the at least one colored ink and the at least one white ink, when an integer greater than or equal to 2 is set as n, the difference [AB] of the ink applied in the nth order becomes the same value or greater than the difference [AB] of the ink applied in the (n-1)th order, and the difference [AB] of the last applied ink is greater than the difference [AB] of the first applied ink.

Citation Information

Patent Citations

  • Pouch

    JP1979004669A

  • Exhaust gas recirculation controller

    JP1979030316A

  • Recording method and device therefor

    JP1979059936A

  • Induction missile

    JP1983063600A

  • Color image forming method

    JP1984157636A