Preparation method of high-strength 7-series aluminum alloy sheet
The preparation process of 7-series aluminum alloy thin sheets was optimized by deformation heat treatment, which solved the problems of high energy consumption and long process of traditional processes. This resulted in aluminum alloy thin sheets with high strength, high plasticity and corrosion resistance, which are suitable for rail transportation and automotive fields.
Patent Information
- Application Number
- CN202410497617.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-24
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-04-24
AI Technical Summary
Traditional aluminum alloy sheet preparation processes are lengthy, energy-intensive, polluting, and require significant equipment investment, resulting in low yields. This hinders their application in rail transportation and automotive sectors, and short-process preparation technologies for 7-series aluminum alloys are scarce.
The deformation heat treatment process, including asynchronous hot rolling, online asynchronous warm rolling, rapid solution treatment, cold rolling, two-stage strengthening solution treatment, and peak aging treatment, optimizes the microstructure of aluminum alloy thin plates. Asynchronous hot rolling breaks up the crystalline phase, rapid solution treatment achieves element homogenization, cold rolling and strengthening solution treatment refine the grains, and finally peak aging treatment is performed.
The aluminum alloy sheet significantly shortens the preparation time and has fine grains, uniform element distribution and weak cube-ND texture, which improves its strength, plasticity and resistance to intergranular corrosion, increases yield strength and tensile strength and elongation.
Smart Images

Figure HDA0004807689950000011 
Figure HDA0004807689950000012 
Figure HDA0004807689950000013
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of aluminum alloy thin sheets, and particularly relates to a method for preparing high-strength 7-series aluminum alloy thin sheets. Background Technology
[0002] Energy consumption, environmental pollution, and carbon emissions are significant global challenges. In sectors such as rail transportation and automobiles, lightweighting has become a crucial measure for addressing these issues. 7-series aluminum alloys, due to their advantages such as low density, high strength and toughness, good fatigue performance, corrosion resistance, and weldability, are gradually becoming important lightweight materials in the rail transportation and automotive industries.
[0003] However, the traditional manufacturing process of aluminum alloy sheets mainly includes casting, homogenization treatment, sawing, milling, hot rough rolling, hot finish rolling, intermediate annealing, cold rolling, and final solution aging treatment. Clearly, traditional manufacturing processes have disadvantages such as long process flow, high energy consumption, large pollution emissions, high equipment investment, and low yield, significantly increasing the manufacturing cost of aluminum alloy sheets and severely hindering their application in related fields.
[0004] Short-process manufacturing is an important way to solve the above problems. Invention patents with publication numbers CN202210309276.2, CN201410708568.9, CN201810073537.9, CN202110834144.7, and CN202110816126.6 introduce short-process manufacturing methods and deformation heat treatment processes for aluminum alloy sheets and strips. However, these patents are all based on process route optimization of traditional casting methods, and short-process manufacturing processes for 7-series aluminum alloys are still relatively scarce. Summary of the Invention
[0005] In view of this, the purpose of the present invention is to provide a method for preparing high-strength 7-series aluminum alloy thin plates. The deformation heat treatment process used in this method significantly shortens the preparation time. The 7-series aluminum alloy thin plates have microstructure characteristics such as fine grain structure, high solid solution, uniform element distribution and weak Cube-ND texture (reducing mechanical anisotropy), and thus obtain higher strength, plasticity and resistance to intergranular corrosion.
[0006] This invention provides a method for preparing high-strength 7-series aluminum alloy thin plates, comprising the following steps:
[0007] After asynchronous hot rolling of 7-series aluminum alloy slabs at 450–470℃, they are cooled to 200–300℃ for online asynchronous warm rolling and cooling; the speed ratio of the upper and lower rolls during asynchronous rolling is 1.2–1.4.
[0008] The cooled slab is subjected to rapid solution treatment, including: holding at 465-475℃ and then cooling to 380-420℃ at a cooling rate of 9-11℃ / min, and then cooling to room temperature at a rate of 2-5℃ / min.
[0009] The slab after rapid solution treatment is cold rolled, followed by two-stage strengthening solution treatment.
[0010] The slab after strengthening and solution treatment is quenched and then subjected to peak aging treatment to obtain a high-strength 7-series aluminum alloy sheet.
[0011] Preferably, the asynchronous hot rolling has a reduction of 40-50% and is performed in three passes.
[0012] Preferably, the reduction in asynchronous warm rolling is 25-30%, and it is done in one pass.
[0013] Preferably, the cold rolling reduction is 45-65%, and the rolling is performed in four passes.
[0014] Preferably, the two-stage enhanced solid solution includes:
[0015] Keep warm at 470–475℃ for 1–2 hours, then keep warm at 480–490℃ for 0.5–1 hour.
[0016] Preferably, the cooling rate is controlled in the furnace after rapid solution treatment.
[0017] Preferably, the quenching method is water cooling;
[0018] Quench to room temperature.
[0019] Preferably, the temperature difference within the furnace during rapid solution treatment and enhanced solution treatment is < ±3℃.
[0020] Preferably, the peak aging treatment temperature is 110–130°C, and the holding time is 22–26 h.
[0021] This invention provides a method for preparing high-strength 7-series aluminum alloy thin plates, comprising the following steps: asynchronous hot rolling of a 7-series aluminum alloy slab at 450–470°C, followed by online asynchronous warm rolling at 200–300°C and further cooling; the speed ratio of the upper and lower rolls during asynchronous rolling is 1.2–1.4; rapid solution treatment of the cooled slab, including: holding at 465–475°C and then cooling at a rate of 9–11°C / min to 380–420°C, followed by cooling at a rate of 2–5°C / min to room temperature; cold rolling of the rapidly solution-treated slab, followed by two-stage strengthening solution treatment; quenching of the strengthened solution-treated slab, and finally peak aging treatment to obtain a high-strength 7-series aluminum alloy thin plate. This method utilizes a deformation heat treatment process that significantly shortens the preparation time; the 7-series aluminum alloy thin plate possesses microstructural characteristics such as fine grain structure, high solid solution, uniform elemental distribution, and weak Cube-ND texture (reducing mechanical anisotropy), resulting in higher strength, plasticity, and resistance to intergranular corrosion. Experimental results show that compared with the traditional process (Comparative Example 1), the preparation cycle of the present invention is shortened by more than 40%; the yield strength of the 7-series aluminum alloy sheet is 478-486 MPa, the tensile strength is 547-553 MPa, the elongation is 12.2-13.2%, and the maximum intergranular corrosion depth is 83-90 μm. Attached Figure Description
[0022] Figure 1 This is a flow chart of the deformation heat treatment process for the high-strength 7-series aluminum alloy sheet in this invention.
[0023] Figure 2 This is a crystalline phase distribution diagram of the raw material slab in Example 1 of the present invention;
[0024] Figure 3 The precipitate distribution diagram is shown for the final aged state sample of the high-strength 7-series aluminum alloy thin sheet prepared in Example 1 of this invention.
[0025] Figure 4 This is a typical grain structure of the final aged state sample of the high-strength 7-series aluminum alloy thin plate prepared in Example 1 of the present invention;
[0026] Figure 5 This is a typical texture of the final aged state sample of the high-strength 7-series aluminum alloy sheet prepared in Example 1 of the present invention;
[0027] Figure 6 The images show typical tensile fracture surfaces of aluminum alloy sheets prepared in Example 1 and Comparative Example 1 of this invention. Detailed Implementation
[0028] This invention provides a method for preparing high-strength 7-series aluminum alloy thin plates, comprising the following steps:
[0029] After asynchronous hot rolling of 7-series aluminum alloy slabs at 450–470℃, they are cooled to 200–300℃ for online asynchronous warm rolling and cooling; the speed ratio of the upper and lower rolls during asynchronous rolling is 1.2–1.4.
[0030] The cooled slab is subjected to rapid solution treatment, including: holding at 465-475℃ and then cooling to 380-420℃ at a cooling rate of 9-11℃ / min, and then cooling to room temperature at a rate of 2-5℃ / min.
[0031] The slab after rapid solution treatment is cold rolled, followed by two-stage strengthening solution treatment.
[0032] The slab after strengthening and solution treatment is quenched and then subjected to peak aging treatment to obtain a high-strength 7-series aluminum alloy sheet.
[0033] Figure 1 This is a flow chart of the deformation heat treatment process for high-strength 7-series aluminum alloy thin plates in this invention; from Figure 1 It can be seen that the deformation heat treatment process generally includes: asynchronous hot rolling + online asynchronous warm rolling - first rapid solution treatment + slow cooling - cold rolling - second solution treatment (two-stage strengthening solution) - aging treatment (peak aging).
[0034] This invention involves asynchronous hot rolling of 7-series aluminum alloy (i.e., Al-Zn-Mg-Cu alloy) slabs at 450–470°C, followed by online asynchronous warm rolling at 200–300°C and subsequent cooling. Preferably, the Al-Zn-Mg-Cu alloy slabs in this invention are prepared according to the following method:
[0035] The 7-series aluminum alloy slab was obtained by melting Zn 5.3-5.6 wt%, Mg 2.0-2.2 wt%, Cu 1.1-1.3 wt%, and the balance Al.
[0036] The present invention preferably involves melting pure Al, pure Zn, and Al50Cu master alloy at a melting temperature of 720–740°C. After complete melting, pure Mg is added, the mixture is allowed to stand, C2Cl6 is added to remove slag and gas, and the mixture is then cast to obtain a 7-series aluminum alloy slab.
[0037] In this invention, after slag and gas removal, the melt is slowly cooled to 720°C, and then the molten aluminum is poured into a mold. During the casting process, it solidifies into a completely solid phase. The cooling rate during casting is 20K / s to 100K / s. This invention describes the cooling rate from the liquid phase to solidification during the casting and solidification process. The 7-series aluminum alloy slab in this invention has a dense and fine solidified structure, with a secondary dendrite spacing <20μm and an average width of the solidified crystalline phase <3μm. The thickness of the 7-series aluminum alloy slab is 6–8mm.
[0038] The present invention performs rapid solution treatment on the cooled slab. The rapid solution treatment includes: holding at 465-475°C and then cooling at a cooling rate of 9-11°C / min to 380-420°C, and then cooling at a cooling rate of 2-5°C / min to room temperature.
[0039] This invention employs asynchronous hot rolling with a speed ratio of 1.2 to 1.4 between the upper and lower rolls; specifically, the speed ratio is 1.2, 1.3, or 1.4. If the asynchronous speed ratio is too small, it is difficult to achieve the effect of asynchronous rolling, similar to traditional synchronous hot rolling; if the asynchronous speed ratio is too large, the sheet is prone to bending and cracking. The reduction in the asynchronous hot rolling is 40-50%, and it is rolled in three passes. This invention eliminates solidification defects through large reduction deformation; utilizes asynchronous hot rolling to break up and refine relatively coarse crystalline phases, reducing element diffusion distance; and obtains deformation energy storage through asynchronous hot rolling, especially deformation energy storage around the crystalline phase, providing energy for recrystallization during the intermediate short-term homogenization process. This invention provides online monitoring of the slab temperature after asynchronous hot rolling. When the slab cools to 200–300°C, online asynchronous warm rolling is performed using the residual heat of the slab, saving energy and reducing processing steps. Compared to asynchronous hot rolling, the rolling temperature is lower, which is more conducive to breaking down and refining the crystalline phase, while also reducing the risk of plate cracking. The reduction in asynchronous warm rolling is 25–30%, and the rolling is completed in one pass. Air cooling is used to cool the slab to room temperature.
[0040] This invention performs rapid solution treatment on cooled slabs, comprising: holding at 465–475°C, then cooling to 380–420°C at a cooling rate of 9–11°C / min, and then cooling to room temperature at a cooling rate of 2–5°C / min. Preferably, the holding time is 0.5–1.5 hours at 465–475°C. After the holding time, the slab is cooled to 380–420°C at a cooling rate of 9–11°C / min, and then cooled to room temperature at a cooling rate of 2–5°C / min. In a specific embodiment, after the holding time, the slab is cooled to 400°C at a cooling rate of 10°C / min. In a specific embodiment, the slab is cooled to room temperature at a rate of 2°C / min; or at 3°C / min; or at 4°C / min; or at 5°C / min. In the rapid solution treatment, most of the already broken and refined crystalline phases are rapidly dissolved, and elemental homogenization and diffusion occur; rapid recrystallization occurs, refining the grains; and precipitates such as MgZn2 are formed during slow cooling (9-11℃ / min cooling rate), increasing the energy storage of cold rolling deformation and enhancing the particle-induced nucleation effect during the final strengthening solution treatment.
[0041] This invention involves cold rolling a slab after rapid solution treatment, followed by a two-stage strengthening solution treatment. The cold rolling reduction is 45%–65%, performed in four passes. The final thickness of the cold-rolled sheet is 1–1.2 mm. In specific embodiments, the cold rolling reduction is 64%, 60%, or 65%. This invention achieves the required final sheet thickness through cold rolling, further breaking down coarse crystalline phases during the cold rolling process, providing deformation energy storage for final solution recrystallization.
[0042] The two-stage enhanced solid solution treatment described in this invention includes: holding at 470–475°C for 1–2 hours, followed by holding at 480–490°C for 0.5–1 hour. This invention achieves complete resolution of the precipitated phase and undissolved crystalline phase through a two-stage enhanced solid solution treatment, completing elemental homogenization and diffusion to obtain a high-solid-solution composition. Utilizing the precipitated phase and undissolved crystalline phase after the first solid solution treatment (rapid solid solution treatment), a large number of particles undergo excited nucleation around the second phase, producing a weaker Cube-ND texture and refining the grains. In the two-stage enhanced solid solution treatment, the 470–475°C stage promotes the dissolution of most low-melting-point crystalline phases, preventing overheating. The subsequent holding at 480–490°C further increases the solubility of the crystalline phase and promotes the aging precipitation process. In a specific embodiment, the two-stage enhanced solution treatment involves first holding the solution at 475°C for 2 hours, then raising the temperature to 485°C and holding it for 0.5 hours; or first holding the solution at 470°C for 2 hours, then raising the temperature to 480°C and holding it for 1 hour; or first holding the solution at 475°C for 1.5 hours, then raising the temperature to 485°C and holding it for 0.5 hours; or first holding the solution at 475°C for 2 hours, then raising the temperature to 485°C and holding it for 1 hour; or first holding the solution at 475°C for 1 hour, then raising the temperature to 490°C and holding it for 0.5 hours.
[0043] After two-stage solution treatment, quenching is performed; water cooling is preferred. Quenching to room temperature requires a sample transfer time of less than 3 seconds. The temperature difference within the furnace during rapid and enhanced solution treatments should be < ±3℃.
[0044] This invention involves quenching a solution-strengthened slab and then performing a peak-aging treatment to obtain a high-strength 7-series aluminum alloy sheet. The peak-aging treatment induces the re-precipitation of nano-precipitates from the highly solution-solidified matrix in the solution-solid state, resulting in precipitation strengthening. The peak-aging treatment temperature is 110–130°C, and the holding time is 22–26 hours. In a specific embodiment, the peak-aging treatment temperature is 120°C, and the holding time is 24 hours.
[0045] The present invention preferably involves cooling to room temperature in air after peak aging treatment. The dwell time between quenching and peak aging treatment is less than 5 minutes.
[0046] In the process described above, the crystalline phase and the precipitated phase can be collectively referred to as the second phase.
[0047] The preparation method provided by this invention involves deformation heat treatment of 7-series aluminum alloy slabs, including asynchronous hot rolling + online asynchronous warm rolling - rapid solution treatment (slow cooling) - cold rolling - two-stage strengthening solution treatment (water quenching) - aging, which can significantly shorten the preparation time. The above deformation heat treatment process fully utilizes the characteristics of (sub)rapid solidification, achieving rapid crystallization re-dissolution, uniform element distribution, grain refinement, and weakening of texture orientation density and optimization of texture type (weak Cube-ND texture, reducing mechanical anisotropy). This short-process deformation heat treatment process simultaneously improves the yield strength, tensile strength, elongation, and intergranular corrosion resistance of 7-series aluminum alloy thin plates, and the matching degree of strength and corrosion resistance can be further optimized by adjusting the aging regime. This deformation heat treatment process is also applicable to other heat-treatable aluminum alloys with (sub)rapid solidification characteristics, requiring only appropriate adjustment of process parameters.
[0048] To further illustrate the present invention, the following detailed description of a method for preparing a high-strength 7-series aluminum alloy sheet provided by the present invention is provided in conjunction with embodiments, but these descriptions should not be construed as limiting the scope of protection of the present invention.
[0049] Preliminary example
[0050] Pure Al, pure Zn, and an Al-50% Cu master alloy were smelted at 730℃. After all metals were completely melted, pure Mg was added. After standing for a period of time, C2Cl6 was added to remove slag and gas for 10 minutes. Finally, when the melt was slowly cooled to 720℃, the molten aluminum was poured into a rapid cooling mold and cooled at a solidification cooling rate of 62K / s to obtain an Al-Zn-Mg-Cu alloy slab with a thickness of 7mm.
[0051] Example 1
[0052] The Al-Zn-Mg-Cu alloy slab prepared in the preliminary example was asynchronously hot rolled at 470℃ with a reduction of 45%, then cooled to 200℃ for online asynchronous warm rolling with a reduction of 28%, and then cooled again; the speed ratio of the upper and lower rolls during asynchronous rolling was 1.3.
[0053] The cooled slab is subjected to rapid solution treatment, including: holding at 470℃ for 1 hour, then cooling to 400℃ at a cooling rate of 10℃ / min, and then cooling to room temperature at a cooling rate of 2℃ / min.
[0054] The slab after rapid solution treatment was cold rolled with a reduction of 64%, and then subjected to two-stage strengthening solution treatment: first, it was held at 475℃ for 2 hours, and then the temperature was raised to 485℃ and held for 0.5 hours.
[0055] After the strengthened solution-treated slab is cooled to room temperature by water, it is immediately subjected to peak aging treatment at 120°C for 24 hours. After aging, it is cooled to room temperature in air to obtain a high-strength 7-series aluminum alloy sheet with a thickness of 1 mm.
[0056] Example 2
[0057] The Al-Zn-Mg-Cu alloy slab prepared in the preliminary example was asynchronously hot rolled at 450°C with a reduction of 45%, then cooled to 200°C for online asynchronous warm rolling with a reduction of 28%, followed by cooling; the speed ratio of the upper and lower rolls during asynchronous rolling was 1.4.
[0058] The cooled slab is subjected to rapid solution treatment, including: holding at 475℃ for 1.5h, then cooling to 400℃ at a cooling rate of 10℃ / min, and then cooling to room temperature at a cooling rate of 5℃ / min.
[0059] The slab after rapid solution treatment was cold rolled with a reduction of 64%, and then subjected to two-stage strengthening solution treatment: first, it was held at 475℃ for 2 hours, and then the temperature was raised to 485℃ and held for 0.5 hours.
[0060] After the strengthened solution-treated slab is cooled to room temperature by water, it is immediately subjected to peak aging treatment at 120°C for 24 hours. After aging, it is cooled to room temperature in air to obtain a high-strength 7-series aluminum alloy sheet with a thickness of 1 mm.
[0061] Example 3
[0062] The Al-Zn-Mg-Cu alloy slab prepared in the preliminary example was asynchronously hot rolled at 465℃ with a reduction of 50%, then cooled to 200℃ for online asynchronous warm rolling with a reduction of 25%, followed by cooling; the speed ratio of the upper and lower rolls during asynchronous rolling was 1.2.
[0063] The cooled slab is subjected to rapid solution treatment, including: holding at 470℃ for 1.5h, cooling to 400℃ at a cooling rate of 10℃ / min, and then cooling to room temperature at a cooling rate of 2℃ / min.
[0064] The slab after rapid solution treatment is cold rolled with a reduction of 60%, and then subjected to two-stage strengthening solution treatment: first, it is held at 470℃ for 2 hours, and then the temperature is raised to 480℃ and held for 1 hour.
[0065] After the strengthened solution-treated slab was water-cooled to room temperature, it was immediately subjected to peak aging treatment at 120℃ for 24 hours. After aging, it was cooled to room temperature in air to obtain a high-strength 7-series aluminum alloy sheet with a thickness of 1.05 mm.
[0066] Example 4
[0067] The Al-Zn-Mg-Cu alloy slab prepared in the preliminary example was asynchronously hot rolled at 460℃ with a reduction of 40%, then cooled to 250℃ for online asynchronous warm rolling with a reduction of 27%, followed by cooling; the speed ratio of the upper and lower rolls during asynchronous rolling was 1.3.
[0068] The cooled slab is subjected to rapid solution treatment, including: holding at 475℃ for 1 hour, then cooling to 400℃ at a cooling rate of 10℃ / min, and then cooling to room temperature at a cooling rate of 3℃ / min.
[0069] The slab after rapid solution treatment is cold rolled with a reduction of 65%, and then subjected to two-stage strengthening solution treatment: first, it is held at 475℃ for 1.5h, and then the temperature is raised to 485℃ and held for 0.5h.
[0070] After the strengthened solution-treated slab was water-cooled to room temperature, it was immediately subjected to peak aging treatment at 120℃ for 24 hours. After aging, it was cooled to room temperature in air to obtain a high-strength 7-series aluminum alloy sheet with a thickness of 1.07 mm.
[0071] Example 5
[0072] The Al-Zn-Mg-Cu alloy slab prepared in the preliminary example was asynchronously hot rolled at 460℃ with a reduction of 50%, then cooled to 300℃ for online asynchronous warm rolling with a reduction of 25%, and then cooled again; the speed ratio of the upper and lower rolls during asynchronous rolling was 1.3.
[0073] The cooled slab is subjected to rapid solution treatment, including: holding at 475℃ for 0.5h, cooling to 400℃ at a cooling rate of 10℃ / min, and then cooling to room temperature at a cooling rate of 2℃ / min.
[0074] The slab after rapid solution treatment is cold rolled with a reduction of 60%, and then subjected to two-stage strengthening solution treatment: first, it is held at 475℃ for 2 hours, and then the temperature is raised to 485℃ and held for 1 hour.
[0075] After the strengthened solution-treated slab was water-cooled to room temperature, it was immediately subjected to peak aging treatment at 120℃ for 24 hours. After aging, it was cooled to room temperature in air to obtain a high-strength 7-series aluminum alloy sheet with a thickness of 1.05 mm.
[0076] Example 6
[0077] The Al-Zn-Mg-Cu alloy slab prepared in the preliminary example was asynchronously hot rolled at 465℃ with a reduction of 45%, then cooled to 200℃ for online asynchronous warm rolling with a reduction of 28%, and then cooled; the speed ratio of the upper and lower rolls during asynchronous rolling was 1.4.
[0078] The cooled slab is subjected to rapid solution treatment, including: holding at 475℃ for 1 hour, then cooling to 400℃ at a cooling rate of 10℃ / min, and then cooling to room temperature at a cooling rate of 2℃ / min.
[0079] The slab after rapid solution treatment was cold rolled with a reduction of 64%, and then subjected to two-stage strengthening solution treatment: first, it was held at 475℃ for 1 hour, and then the temperature was raised to 490℃ and held for 0.5 hours.
[0080] After the strengthened solution-treated slab is cooled to room temperature by water, it is immediately subjected to peak aging treatment at 120°C for 24 hours. After aging, it is cooled to room temperature in air to obtain a high-strength 7-series aluminum alloy sheet with a thickness of 1 mm.
[0081] Comparative Example 1 (Traditional Preparation Process)
[0082] 1) The Al-Zn-Mg-Cu alloy slab prepared in the preliminary example was homogenized: held at 470℃ for 24h and cooled to room temperature at 5℃ / min;
[0083] 2) Hot rolling: The hot rolling temperature is 420℃, and the hot rolling deformation is 62.5%;
[0084] 3) Intermediate annealing: Annealing temperature is 420℃, and the holding time is 2 hours;
[0085] 4) Cold rolling: Cold rolled to 1.2mm, with a cold rolling deformation of 60%;
[0086] 5) Solution hardening treatment: Hold at 470℃ for 2 hours, then rapidly quench (water cool) to room temperature;
[0087] 6) Peak aging treatment: After solution quenching, immediately hold at 120℃ for 24 hours, and then cool to room temperature in air after aging.
[0088] Comparative Example 2
[0089] 1) The Al-Zn-Mg-Cu alloy slab prepared in the preliminary example was simultaneously hot rolled: the hot rolling holding temperature was 470℃, the hot rolling deformation was 62.5%, and the upper and lower rolls rotated at the same speed;
[0090] 2) First rapid solution treatment (without slow cooling): Hold at 470℃ for 1.5h, then rapidly cool to room temperature by water cooling;
[0091] 3) Cold rolling: Cold rolled to 1.2mm, with a cold rolling deformation of 60%;
[0092] 4) Second solution treatment: Hold at 470℃ for 2 hours, then rapidly quench (water cool) to room temperature;
[0093] 5) Peak aging treatment: After solution quenching, immediately hold at 120℃ for 24 hours (peak aging), and then cool to room temperature in air.
[0094] Comparative Example 3
[0095] 1) The Al-Zn-Mg-Cu alloy slab prepared in the preliminary example was asynchronously hot rolled: the hot rolling holding temperature was 470℃, the hot rolling deformation was 62.5%, and the speed ratio of the upper and lower rolls was 1.3;
[0096] 2) First rapid solution treatment (without slow cooling): Hold at 470℃ for 1.5h, then rapidly cool to room temperature by water cooling;
[0097] 3) Cold rolling: Cold rolled to 1.2mm, with a cold rolling deformation of 60%;
[0098] 4) Second solution treatment: Hold at 470℃ for 2 hours, then rapidly quench (water cool) to room temperature;
[0099] 5) Peak aging treatment: After solution quenching, immediately hold at 120℃ for 24 hours (peak aging), and then cool to room temperature in air.
[0100] Comparative Example 4
[0101] 1) The Al-Zn-Mg-Cu alloy slab prepared in the preliminary example was asynchronously hot rolled: the hot rolling holding temperature was 470℃, the hot rolling deformation was 62.5%, and the speed ratio of the upper and lower rolls was 1.3;
[0102] 2) First rapid solution treatment (without slow cooling): Hold at 470℃ for 1.5h, then rapidly cool to room temperature by water cooling;
[0103] 3) Cold rolling: Cold rolled to 1.2mm, with a cold rolling deformation of 60%;
[0104] 4) Second solution treatment (including strengthening solution treatment): Hold at 470℃ for 2 hours, then hold at 485℃ for 1 hour, and finally quench (water cool) to room temperature.
[0105] 5) Peak aging treatment: After solution quenching, immediately hold at 120℃ for 24 hours (peak aging), and then cool to room temperature in air.
[0106] Comparative Example 5
[0107] 1) The Al-Zn-Mg-Cu alloy slab prepared in the preliminary example was asynchronously hot-rolled and then asynchronously warm-rolled online: the hot rolling holding temperature was 470℃, the hot rolling deformation was 45%, and the plate was cooled to about 300℃ for online warm rolling with a reduction of 28% and the speed ratio of the upper and lower rolls was 1.3.
[0108] 2) First rapid solution treatment (without slow cooling): Hold at 470℃ for 1.5h, then rapidly cool to room temperature by water cooling;
[0109] 3) Cold rolling: Cold rolled to 1.2mm, with a cold rolling deformation of 60%;
[0110] 4) Second solution treatment (including strengthening solution treatment): Hold at 470℃ for 2 hours, then hold at 485℃ for 1 hour, and finally quench (water cool) to room temperature.
[0111] 5) Peak aging treatment: After solution quenching, immediately hold at 120℃ for 24 hours (peak aging), and then cool to room temperature in air.
[0112] The intergranular corrosion test and detection method of the high-strength 7-series aluminum alloy thin plate prepared in this invention is described in GB / T 7998-200 "Method for Determination of Intergranular Corrosion of Aluminum Alloys".
[0113] Table 1. Mechanical properties and intergranular corrosion resistance of the embodiments and comparative examples of the present invention.
[0114] Case Yield strength / MPa Tensile strength / MPa Elongation / % Maximum intergranular corrosion depth / μm Example 1 485 553 13.2 86 Example 2 478 547 13.0 88 Example 3 483 550 12.8 89 Example 4 486 552 12.5 83 Example 5 480 552 13.6 84 Example 6 482 551 12.2 90 Comparative Example 1 462 520 10.2 98 Comparative Example 2 470 533 11.8 92 Comparative Example 3 478 540 11.2 96 Comparative Example 4 482 546 12.0 93 Comparative Example 5 476 543 12.4 101
[0115] Note: The smaller the maximum intergranular corrosion depth, the higher the resistance to intergranular corrosion.
[0116] It should be noted that the process in Comparative Example 2 can be applied to thin-strip continuous casting Al-Zn-Mg-Cu alloys with sub-rapid solidification characteristics ("Study on Microstructure and Properties of Electromagnetically Cast Al-Zn-Mg-Cu Alloys Based on Short-Process Heat Treatment"), but its overall performance is far lower than that of the deformation heat treatment process of this invention, especially in terms of strength. To compensate for the shortcomings of the process in Comparative Example 2, based on the principle of microalloying, high-strength Al-Zn-Mg-Cu-Zr-Sc alloy thin plates can also be obtained by adding excess Sc and Zr elements to refine the as-cast grains and crystalline phase sizes. However, to enhance the precipitation strengthening effect of Sc and Zr, a long-term low-temperature pretreatment (300℃-24h) is required on the basis of Comparative Example 2, resulting in a long preparation time. Sc is a precious metal, leading to high costs. Microstructurally, the Al-Zn-Mg-Cu-Sc-Zr alloy inhibits recrystallization and grain growth through a large amount of Al3(Sc,Zr) phase, and the T6 state microstructure is dominated by fine deformation, thus improving strength. Its texture is also a deformation texture with a high orientation density, which is not conducive to reducing mechanical anisotropy. This invention, based on the solidification microstructure characteristics of Al-Zn-Mg-Cu alloys, designs and refines the deformation heat treatment process, achieving the following characteristics: fully utilizing the particle-induced nucleation of the second phase to promote recrystallization, refine grains, and ultimately obtain a Cube-ND texture with a weak orientation density and fine grains, improving plasticity and reducing mechanical anisotropy; the second phase dissolves more completely, enhancing precipitation strengthening ability; and high-strength aluminum-plastic alloy thin plates are obtained.
[0117] As can be seen from the above embodiments, the present invention provides a method for preparing high-strength 7-series aluminum alloy thin plates, comprising the following steps: asynchronous hot rolling of 7-series aluminum alloy slabs at 450-470℃, followed by cooling to 200-300℃ for online asynchronous warm rolling and cooling; the speed ratio of the upper and lower rolls during asynchronous rolling is 1.2-1.4; rapid solution treatment of the cooled slabs, including: holding at 465-475℃ and then cooling to 380-420℃ at a cooling rate of 9-11℃ / min, followed by cooling to room temperature at a rate of 2-5℃ / min; cold rolling of the rapidly solution-treated slabs, followed by two-stage strengthening solution treatment, and quenching of the strengthened solution-treated slabs; and finally, peak aging treatment to obtain high-strength 7-series aluminum alloy thin plates. The deformation heat treatment process employed in this method significantly shortens the preparation time. The 7-series aluminum alloy thin plates exhibit microstructural characteristics such as fine grain structure, high solid solution, uniform elemental distribution, and weak Cube-ND texture (reducing mechanical anisotropy), resulting in higher strength, plasticity, and resistance to intergranular corrosion. Experimental results show that the preparation cycle is shortened by more than 40%; the yield strength of the 7-series aluminum alloy thin plates is 478–486 MPa, the tensile strength is 547–553 MPa, the elongation is 12.2–13.2%, and the maximum intergranular corrosion depth is 83–90 μm.
[0118] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a high-strength 7-series aluminum alloy thin sheet, comprising the following steps: After asynchronous hot rolling of 7-series aluminum alloy slabs at 450~470℃, they are cooled to 200~300℃ for online asynchronous warm rolling and cooling. The speed ratio of the upper and lower rolls during asynchronous rolling is 1.2~1.
4. The reduction of the asynchronous hot rolling is 40~50%, and it is rolled in three passes. The reduction of the asynchronous warm rolling is 25~30%, and it is rolled in one pass. The cooled slab is subjected to rapid solution treatment, including: holding at 465~475℃ for 0.5~1.5h, cooling to 380~420℃ at a cooling rate of 9~11℃ / min, and then cooling to room temperature at a cooling rate of 2~5℃ / min. The slab after rapid solution treatment is cold rolled, followed by two-stage strengthening solution treatment; the cold rolling reduction is 45-65%, and it is rolled in four passes. The two-stage enhanced solution treatment includes: holding at 470~475℃ for 1~2 h, followed by holding at 480~490℃ for 0.5~1 h; During rapid solution treatment and enhanced solution treatment, the temperature difference within the furnace is < ±3℃. The slab after strengthening and solution treatment is quenched and then subjected to peak aging treatment to obtain high-strength 7-series aluminum alloy thin plate. The peak aging treatment temperature is 110~130℃, and the holding time is 22~26h.
2. The preparation method according to claim 1, characterized in that, The cooling rate is controlled in the furnace after rapid solution treatment.
3. The preparation method according to claim 1, characterized in that, The quenching method is water cooling; quench to room temperature.
Citation Information
Patent Citations
Short process preparation method of 6xxx series aluminum alloy body panel without paint brush line
CN104532077B
A short-process deformation heat treatment method for preparing high-strength and corrosion-resistant Al-Mg-Zn aluminum alloys
CN108359920B
A short-process, high-conductivity 6-series aluminum alloy sheet and strip and its preparation method
CN113528900B
Thermomechanical treatment method for preparing high-strength and high-corrosion-resistance Al-Mg-Zn aluminum alloy in short process
CN113699396A