Method for casting 6t rectangular ingot
By designing the casting cavity of the 6t rectangular steel ingot mold as a rectangular neck-reduced and elongated structure, the problem of component segregation during the solidification process of raw steel was solved. Furthermore, by heating in a continuous heating furnace, the yield and resource utilization efficiency were improved.
Patent Information
- Application Number
- CN202410425417.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-09
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-04-09
Smart Images

Figure CN118305277B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the technical field of raw material steel ingot casting, and more specifically, to a method for casting a 6t rectangular steel ingot. Background Technology
[0002] Please refer to Figures 1 to 5 ,in, Figure 1 This is a schematic diagram of the structure of a 3t square steel ingot mold in the prior art; Figure 2 This is a schematic diagram of the structure of a 3t steel ingot in the head direction in the existing technology; Figure 3 This is a schematic diagram of the structure of a 3t steel ingot in the tail direction in the prior art; Figure 4 A flow chart of the production process of raw steel for vacuum induction furnaces in the existing technology; Figure 5 A comparative diagram illustrating the rolling processes of steel ingots and continuously cast billets in existing technologies.
[0003] Raw material steel is the main raw material used in vacuum induction furnace steelmaking. It is an iron-carbon alloy with a lower alloy content compared to conventional steel grades. Since raw material steel is used as a feedstock for vacuum induction furnaces, the main requirements for smelting quality control are that the composition meets standard requirements and that all inclusions have low ratings. The production process of raw material steel is briefly described as follows: Before casting molten steel, six 3t square steel ingot molds (e.g., ...) are placed on a base plate. Figure 1 (As shown); the molten raw steel is poured into a 3t ingot mold using the bottom pouring method to form a 3t ingot (as shown). Figures 2-3 After the raw steel is cast, it is heated and rolled in a steel rolling mill to form small-sized round steel bars (Ф40mm, Ф75mm, Ф85mm, Ф95mm, etc.). Then, it can be sheared to obtain small pieces of material with a length of about 190-240mm to be put into the furnace.
[0004] In existing technology, the 3t steel ingot mold and its matching risers used in the production of raw material steel are of a split structure, with a large riser volume ratio of approximately 18% (the specific dimensions of the 3t square steel ingot are shown in Table 1). The production process of raw material steel for vacuum induction furnaces is as follows: Figure 4 As shown.
[0005] Table 1 In existing rolling technologies, both ingot castings and continuously cast billets require heating before rolling. The purpose of heating is to increase the temperature of the billet, improve its plasticity, reduce its resistance to deformation, and facilitate rolling. Existing heating methods are divided into soaking furnace heating and continuous heating furnace heating. Soaking furnaces are mainly used for heating steel ingots. Their heating method differs from continuous heating furnaces; it is intermittent heating. That is, after the steel ingot is removed from the furnace, the furnace temperature is lowered again, and then ingots at room temperature or low temperature are placed in for reheating and holding. In actual production, the heating time for one batch of steel is 10-20 hours. Soaking furnace heating produces steel ingots with uniform temperature, which is better than continuous furnace heating, but its production volume and efficiency are much lower. Figure 5 The diagram shows the rolling process for steel ingots and continuously cast billets.
[0006] The chemical composition control range for a certain grade of raw steel is extremely narrow, as shown in Table 2, which specifies the carbon and sulfur content control requirements for this grade of raw steel. As shown in Table 2 (Table 2 shows the control requirements for heavy carbon and sulfur content of a certain grade of raw steel), the maximum and minimum carbon content in this grade of raw steel has a very small range, only 0.02%, while the sulfur content requirement for this type of raw steel is also very low.
[0007] Table 2 The casting time for a 3t steel ingot is required to be 340-440 seconds. The ingot mold is made of cast iron, which has strong heat transfer capabilities. During normal casting, the molten steel rises steadily within the mold. The high-temperature molten steel mainly transfers heat through the mold bottom and walls. The molten steel near the mold bottom and walls is the first to solidify. The solidification direction of the molten steel within the mold is generally from the mold walls towards the center of the mold, and from the bottom of the mold cavity towards the top. After the molten steel has completely solidified in the mold, it needs to be promptly removed from the mold and the ingot is taken out. According to the empirical formula t=0.11R² (where t is the time for complete solidification of the molten steel in minutes; R is the radius of the ingot in centimeters), the complete solidification time for a 3t square ingot is calculated to be as long as 83 minutes. In addition, the 3t square steel ingots of this grade are heated in a soaking pit before rolling. After being heated in the soaking pit of the steel mill, they are then rolled into billets, and then the steel mill directly produces 40mm round steel (round steel with a diameter of 40mm). The yield rate can generally reach 80.5%.
[0008] The shortcomings and deficiencies of existing technologies are summarized as follows: 1. The soaking furnace resources in steel rolling mills are extremely strained. In reality, the raw steel is only intended for use in vacuum induction furnaces, serving as feedstock for remelting. The smelting and casting stages only require ensuring the composition and cleanliness. The purpose of rolling the raw steel is merely to make its specifications meet the requirements of the vacuum induction furnace stage. There is absolutely no need for the raw steel to be first cast into 3-ton ingots and then heated in the soaking pit, as is done with ordinary grades. The existing rolling process for a certain grade of raw steel uses the same ingot rolling process to produce a simple grade, consuming a large amount of valuable soaking furnace resources.
[0009] 2. Current smelting technology can ensure that the carbon and sulfur content of the raw steel of this grade meets the standard requirements at the end of refining. However, the cross-sectional dimensions of the 3t steel ingot mold are relatively large, and component segregation is prone to occur along the solidification direction when the molten steel solidifies in the mold to form the ingot. According to the principle of solidification segregation, elements such as carbon and sulfur have higher solubility in liquid than in solid. At the front of solidification, carbon and sulfur elements will accumulate in the molten steel, resulting in a higher content in the liquid than in the solid. The longer the solidification time and the slower the solidification rate, the greater the degree of carbon and sulfur segregation. The existing 3t steel ingot casting process is the bottom pouring method. When molten steel is poured into the mold, the molten steel at the bottom and edges of the ingot mold solidifies first, while the molten steel at the top and center of the ingot mold solidifies later. The 3t steel ingot mold has a large inner radius, resulting in a long solidification time and slow solidification rate for the molten steel. Upon completion of solidification, easily segregating elements such as carbon and sulfur tend to accumulate at the large end and riser of the ingot, causing positive segregation at the large end and negative segregation at the small end. Since the carbon and sulfur content control range for this grade of raw steel is very narrow, the carbon and sulfur content of the ingot is very likely to fail to meet standard requirements (as shown in Table 3, which illustrates the component segregation at the large and small ends of a 3t steel ingot of a certain grade of raw steel). Therefore, it is necessary to redesign and develop an ingot mold with a smaller cross-sectional dimension than the 3t square steel ingot mold to reduce component segregation during solidification by shortening the solidification time and increasing the solidification rate.
[0010] Table 3 Summary of the Invention
[0011] (a) Technical issues: In summary, how to provide a novel steel ingot mold structure, in which the raw steel ingots cast using this mold do not need to be heated in the soaking furnace of the steel rolling mill, and in which the carbon and sulfur content of this new ingot type raw steel ingots can meet the requirements of narrow composition range control, has become an urgent problem to be solved by those skilled in the art.
[0012] (II) Technical Solution: To achieve the above objectives, the present invention provides the following technical solution: This invention provides a method for casting a 6t rectangular steel ingot. The method includes: Step 1: Set up a 6t rectangular steel ingot mold for later use. The casting cavity of the 6t rectangular steel ingot mold is a rectangular neck-reduced and elongated cavity structure. The casting cavity of the 6t rectangular steel ingot mold is elongated to not less than 5000mm. At least one pair of side dimensions in the cross-section of the casting cavity of the 6t rectangular steel ingot mold are reduced. The height-to-diameter ratio of the casting cavity of the 6t rectangular steel ingot mold is in the range of 9.5-10.0. Step 2: Install the 6t rectangular steel ingot mold and pour molten steel into the casting cavity of the 6t rectangular steel ingot mold using the pit casting method; Step 3: Demold the steel ingot from the 6t rectangular steel ingot mold, then heat and open the billet.
[0013] Preferably, in the 6t rectangular steel ingot casting method provided by the present invention, in the casting cavity, the size range of one pair of sides is 500mm±20mm, and the size range of the other pair of sides is 370mm±10mm; the taper range of the casting cavity is 0.38%-0.42%.
[0014] Preferably, in the 6t rectangular steel ingot casting method provided by the present invention, in step one, the filler ratio of the 6t rectangular steel ingot cast by the 6t rectangular steel ingot mold is in the range of 8%-10%.
[0015] Preferably, in the 6t rectangular steel ingot casting method provided by the present invention, in step two, after fixing the 6t rectangular steel ingot mold, protective slag is set in the casting cavity of the 6t rectangular steel ingot mold by hanging method.
[0016] Preferably, in the 6t rectangular steel ingot casting method provided by the present invention, protective slag is provided at positions 200±20mm and 500±50mm away from the bottom of the mold in the casting cavity.
[0017] Preferably, in the 6t rectangular steel ingot casting method provided by the present invention, the amount of protective slag used is 2kg / t.
[0018] Preferably, in the 6t rectangular steel ingot casting method provided by the present invention, in step two, when fixing the 6t rectangular steel ingot mold, three 6t rectangular steel ingot molds are set on each base plate.
[0019] Preferably, in the 6t rectangular steel ingot casting method provided by the present invention, the 6t rectangular steel ingot mold is set on the base plate by a chassis.
[0020] Preferably, in the 6t rectangular steel ingot casting method provided by the present invention, in step two, during the process of pouring molten steel into the casting cavity of the 6t rectangular steel ingot mold, the ingot body casting speed is 550-650 seconds, and the riser casting speed is 180-300 seconds.
[0021] Preferably, the 6t rectangular steel ingot casting method provided by the present invention further includes step four, which involves heating the billet after it has been opened and then precision rolling it into a round steel product. The dimensions of the round steel product are: a length of 190mm-240mm and a diameter of 120±5mm.
[0022] Preferably, in the 6t rectangular steel ingot casting method provided by the present invention, in step four, the steel billet is heated in a continuous heating furnace and then precision rolled into a circular steel product.
[0023] Preferably, in the 6t rectangular steel ingot casting method provided by the present invention, in step two, a central injection pipe is set on the base plate, and molten steel is cast by bottom injection through the central injection pipe.
[0024] Preferably, in the 6t rectangular steel ingot casting method provided by the present invention, the central injection pipe is mounted on the base plate with adjustable height via a base.
[0025] Preferably, in the 6t rectangular steel ingot casting method provided by the present invention, a plurality of the 6t rectangular steel ingot molds are arranged at equal intervals around the central injection pipe.
[0026] Preferably, in the 6t rectangular steel ingot casting method provided by the present invention, the top end of the central injection pipe is higher than the top end of the 6t rectangular steel ingot mold, and the height difference is N; N is 8%-12% of the length of the 6t rectangular steel ingot mold.
[0027] (III) Beneficial Effects: This invention provides a method for casting a 6t rectangular steel ingot. The method includes: Step 1, setting up a 6t rectangular steel ingot mold, wherein the casting cavity of the 6t rectangular steel ingot mold is a rectangular necked and elongated cavity structure, the casting cavity of the 6t rectangular steel ingot mold is elongated to not less than 5000mm, at least one pair of side dimensions in the cross-section of the casting cavity of the 6t rectangular steel ingot mold are reduced, and the height-to-diameter ratio of the casting cavity of the 6t rectangular steel ingot mold is in the range of 9.5-10.0; Step 2, installing the 6t rectangular steel ingot mold and pouring molten steel into the casting cavity of the 6t rectangular steel ingot mold using a pit casting method; Step 3, demolding the steel ingot in the 6t rectangular steel ingot mold, then heating and blanking.
[0028] Through the above-described design, the 6t rectangular steel ingot casting method provided by this invention has at least the following beneficial effects: In the 6t raw material steel ingot mold used in this invention, the cross-sectional size of the casting cavity is reduced, and the length of the casting cavity is increased. Compared with the 3t square steel ingot mold, the molten steel solidifies faster in the 6t rectangular steel ingot mold. During solidification in the mold, the molten steel is less prone to component segregation in the solidification direction. Due to the shortened solidification time in the casting cavity, the carbon and sulfur content of the steel ingot meets the standard requirements. Furthermore, because this invention increases the length of the casting cavity, the 6t rectangular raw material steel ingot cast by the 6t rectangular steel ingot mold provided by this invention, although a steel ingot, is relatively long. Therefore, it does not require heating in a soaking pit before rolling, but is heated in a continuous heating furnace in the steel rolling mill before subsequent processing. This effectively utilizes the capacity of the soaking pit in the steel rolling mill. Finally, the present invention saws off the ends of YLG steel ingots of a certain grade produced by a 6t rectangular steel ingot mold and 3t YLG steel ingots after they are finished, and samples are taken for inclusion rating. The inclusion level of the YLG steel ingot of a certain grade produced by the 6t rectangular steel ingot mold is ≤1.5 after it is finished, which is comparable to that of the 3t steel ingot. At the same time, its yield is significantly improved. Attached Figure Description
[0029] The accompanying drawings, which form part of this application, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. Wherein: Figure 1 This is a schematic diagram of the structure of a 3t square steel ingot mold in the prior art; Figure 2 This is a schematic diagram of the structure of a 3t steel ingot in the head direction in the existing technology; Figure 3 This is a schematic diagram of the structure of a 3t steel ingot in the tail direction in the prior art; Figure 4 A flow chart of the production process of raw steel for vacuum induction furnaces in the existing technology; Figure 5 A comparative diagram illustrating the rolling processes of steel ingots and continuously cast billets in existing technologies.
[0030] Figure 6 This is a schematic diagram of the external dimensions of the 6t rectangular steel ingot mold in the embodiment of the present invention from the main viewpoint; Figure 7 This is a schematic diagram of the external dimensions of the 6t rectangular steel ingot mold in an embodiment of the present invention from a side view. Figure 8 This is a schematic diagram of the structure of a 6t rectangular raw material steel ingot in the head direction in an embodiment of the present invention; Figure 9 This is a schematic diagram of the structure of a 6t rectangular raw material steel ingot in the tail direction in an embodiment of the present invention; Figure 10 This is a schematic diagram of Ф120 specification raw material steel in an embodiment of the present invention; Figure 11 This is a process flow diagram of the one-fire forming of rectangular raw steel ingots in an embodiment of the present invention; Figure 12 This is a schematic diagram of the tray arrangement effect of a 6t rectangular steel ingot mold in an embodiment of the present invention.
[0031] All dimensions in the accompanying drawings and the specification list are in millimeters (mm).
[0032] exist Figure 6 , Figure 7 as well as Figure 12 In the diagram, the correspondence between component names and reference numerals is as follows: 6t rectangular steel ingot mold: 1. Casting cavity; 2. Mold bottom hole; 3. Riser structure; 4. Lifting lugs; 5. Base plate; 6. 7. Injection pipe, 8. Base plate, 9. Base. Detailed Implementation
[0033] The present invention will now be described in detail with reference to the accompanying drawings and embodiments. Various examples are provided by way of explanation and not by way of limitation. Indeed, those skilled in the art will recognize that modifications and variations can be made to the invention without departing from its scope or spirit. For example, a feature shown or described as part of one embodiment may be used in another embodiment to produce yet another embodiment. Therefore, it is desirable that the invention encompass such modifications and variations falling within the scope of the appended claims and their equivalents.
[0034] In the description of this invention, the terms "longitudinal," "lateral," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," and "bottom," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing the invention and do not require the invention to be constructed and operated in a specific orientation; therefore, they should not be construed as limitations on the invention. The terms "connected" and "linked" used in this invention should be interpreted broadly. For example, they can refer to a fixed connection or a detachable connection; they can refer to a direct connection or an indirect connection through intermediate components. Those skilled in the art can understand the specific meaning of the above terms according to the specific circumstances.
[0035] Please refer to Figures 6 to 12 ,in, Figure 6 This is a schematic diagram of the external dimensions of the 6t rectangular steel ingot mold in the embodiment of the present invention from the main viewpoint; Figure 7 This is a schematic diagram of the external dimensions of the 6t rectangular steel ingot mold in an embodiment of the present invention from a side view. Figure 8This is a schematic diagram of the structure of a 6t rectangular raw material steel ingot in the head direction in an embodiment of the present invention; Figure 9 This is a schematic diagram of the structure of a 6t rectangular raw material steel ingot in the tail direction in an embodiment of the present invention; Figure 10 This is a schematic diagram of Ф120 specification raw material steel in an embodiment of the present invention; Figure 11 This is a process flow diagram of the one-fire forming of rectangular raw steel ingots in an embodiment of the present invention; Figure 12 This is a schematic diagram of the tray arrangement effect of a 6t rectangular steel ingot mold in an embodiment of the present invention.
[0036] This invention provides a method for casting a 6t rectangular steel ingot, which includes the following steps: Step 1: Set up a 6t rectangular steel ingot mold 1 for later use. The 6t rectangular steel ingot mold 1 is a unique steel ingot mold for casting raw steel, which is an innovation of this invention.
[0037] In one embodiment of the present invention, the 6t rectangular steel ingot mold 1 has a casting cavity 2 with a rectangular cross-section. The cross-sectional area of the upper end of the casting cavity 2 is slightly larger than that of the lower end, thus making the entire casting cavity 2 a conical structure. A mold bottom hole 3 is provided at the bottom of the 6t rectangular steel ingot mold 1. The mold bottom hole 3 is a rectangular hole structure, and its shape is consistent with the bottom shape of the casting cavity 2. Thus, the mold bottom hole 3 and the casting cavity 2 are connected to form a structure with a smooth inner wall side (without bosses, steps, or other structures). A riser structure 4 is provided at the top of the 6t rectangular steel ingot mold 1. The diameter of the riser structure 4 is larger than the diameter of the top of the casting cavity 2. The riser structure 4 is connected to the casting cavity 2 and forms a stepped opening structure with an enlarged opening at the top of the casting cavity 2. A thickened layer is provided on the outside of the 6t rectangular steel ingot mold 1 and near its two ends. A lifting lug 5 is provided on the outside of the 6t rectangular steel ingot mold 1 and near its top. The lifting lug 5 is located on the lower side of the top thickened layer.
[0038] In this invention, the casting cavity 2 of the 6t rectangular steel ingot mold 1 is a rectangular (the cross-section of the casting cavity 2 is rectangular) necked (the cross-sectional area of the casting cavity 2 of the 6t rectangular steel ingot mold 1 of this invention is smaller than the cross-sectional area of the casting cavity of the traditional 3t rectangular steel ingot mold, and compared with the cross-section of the casting cavity of the traditional 3t rectangular steel ingot mold, the dimensions of at least one pair of sides of the casting cavity 2 of the 6t rectangular steel ingot mold 1 of this invention are reduced, while the dimensions of the other pair of sides are not increased) elongated (the length of the casting cavity 2 of the 6t rectangular steel ingot mold 1 of this invention is greater than the length of the casting cavity 2 of the traditional 3t rectangular steel ingot mold) cavity structure.
[0039] The casting cavity 2 of the 6t rectangular steel ingot mold 1 is lengthened to no less than 5000mm (the traditional size is 1670mm). At least one pair of side dimensions in the cross-section of the casting cavity 2 of the 6t rectangular steel ingot mold 1 are reduced, and the height-to-diameter ratio of the casting cavity 2 of the 6t rectangular steel ingot mold 1 is in the range of 9.5-10.0.
[0040] Specifically, in casting cavity 2, the dimensions of one pair of sides range from 500mm ± 20mm, and the dimensions of the other pair of sides range from 370mm ± 10mm; the taper of casting cavity 2 ranges from 0.38% to 0.42%.
[0041] Furthermore, in step one, the filler ratio of the 6t rectangular steel ingot cast by the 6t rectangular steel ingot mold 1 is in the range of 8%-10%.
[0042] Step 2: Install the 6t rectangular steel ingot mold 1 and pour molten steel into the casting cavity 2 of the 6t rectangular steel ingot mold 1 using the pit casting method.
[0043] In step two, after fixing the 6t rectangular steel ingot mold 1, protective slag is placed in the casting cavity 2 of the 6t rectangular steel ingot mold 1 using a hanging method. Protective slag is placed in the casting cavity 2 at positions 200±20mm and 500±50mm from the bottom of the mold. The amount of protective slag used is 2kg / t.
[0044] In this invention, during step two, when fixing the 6t rectangular steel ingot mold 1, three 6t rectangular steel ingot molds 1 are set on each base plate 8. The 6t rectangular steel ingot molds 1 are set on the base plate 8 via a base plate 6. A central injection pipe 7 is set on the base plate 8, and molten steel is poured through the central injection pipe 7 using a bottom-pouring method. The central injection pipe 7 is height-adjustably set on the base plate 8 via a base 9 (multiple bases 9 can be set, or a raised base 9 can be set; both the base 9 and the base plate 6 are installation auxiliary components, the base 9 is used for the installation of the central injection pipe 7, and the base plate 6 is used for the installation of the 6t rectangular steel ingot mold 1). Multiple 6t rectangular steel ingot molds 1 are arranged at equal intervals around the central injection pipe 7. Furthermore, the top of the central injection pipe 7 is higher than the top of the 6t rectangular steel ingot mold 1 by a distance of N; N is 8%-12% of the length of the 6t rectangular steel ingot mold 1. For example, if the length of the 6t rectangular steel ingot mold 1 is 5000mm, then the top of the central injection pipe 7 is 500mm higher than the top of the 6t rectangular steel ingot mold 1.
[0045] Specifically, in step two, during the process of pouring molten steel into the casting cavity 2 of the 6t rectangular steel ingot mold 1, the casting speed of the ingot body is 550-650 seconds, and the casting speed of the riser is 180-300 seconds.
[0046] Step 3: Demold the steel ingot from the 6t rectangular steel ingot mold 1, then heat and open the billet.
[0047] Step four involves heating the billet after it has been opened, followed by precision rolling into round steel bars. The dimensions of the round steel bars are: length between 190mm and 240mm, and diameter between 120±5mm. In step four, the billet is heated in a continuous heating furnace and then precision rolled into round steel bars.
[0048] As described above, this invention provides a 6t rectangular steel ingot mold for casting steel ingots made from raw materials with controlled low-composition ranges. Figure 6 and Figure 7 As shown, the structure of a 6t rectangular steel ingot mold is as follows: The casting process for a 6t rectangular steel ingot according to this invention is as follows: 1. Pit casting (a type of mold casting where the steel ingot mold is placed on a base plate in a casting pit for pouring; the entire pouring operation takes place inside the ingot). A 5-meter small tapered steel ingot with a cross-section of 380×500mm is used. Before pouring, each ingot mold is suspended with protective slag (a method of setting protective slag). Based on the designed ingot weight of 6.5t and the principle of using 2kg / t of protective slag, this ingot type uses 12kg (6 2) The ingots are suspended at heights of 200mm and 500mm from the bottom of the mold, respectively. After demolding, the surface of the ingots must not have significant defects and must meet transfer standards. Three ingots are cast simultaneously from one mold base (i.e., three 6t rectangular ingot molds are set up on one base for simultaneous casting). The ingot body casting speed is 550-650 seconds, and the riser casting speed is 180-300 seconds. The molten steel rises rapidly within the mold, with the molten steel near the base and the mold walls solidifying first.
[0049] 2. The steel ingot is demolded and transferred. The solidification direction of the molten steel within the 6t rectangular steel ingot mold is generally from the mold wall towards the mold center, and from the bottom of the mold cavity towards the top. Calculated using the inspection formula t=0.11R² (where t is the complete solidification time of the molten steel in minutes; R is the radius of the steel ingot in centimeters), the complete solidification time of the ingot body is 68.75 minutes. The 6t rectangular steel ingot mold provided by this invention has a slender inner cavity; therefore, the steel ingot cast using this invention is slender. If demolded at a high temperature, the steel ingot is prone to bending. Therefore, the process specifies a mold cooling time of 20 hours after casting and before demolding. After 20 hours of mold cooling, the surface temperature of the steel ingot is low, effectively preventing bending. The shape of the 6t rectangular steel ingot cast using the 6t rectangular steel ingot mold is as follows: Figure 8 and Figure 9 .
[0050] 3. The 6t rectangular raw steel ingot is heated and rolled in a steel rolling mill. Although the 6t rectangular raw steel ingot, cast using the 6t rectangular ingot mold provided by this invention, is an ingot, its length is relatively large (5m). Therefore, it is not heated in a soaking pit before rolling, but in a continuous heating furnace in the steel rolling mill. Subsequently, it undergoes a 240mm square initial rolling (meaning the cross-sectional shape of the initial rolled billet is square, with a side length of 240mm). Each initial rolling takes approximately 3 minutes. It is then cut in half at a fixed length of 6m (this means that after initial rolling, the entire 6t rectangular steel ingot is cut into 6-meter segments using large shears; the length of the 6t rectangular steel ingot increases after initial rolling, and cutting it into 6-meter segments allows the entire initial rolled billet to be cut into two pieces). Fixed length refers to the specific length of the steel billet and finished steel product as specified in the product standard. Producing products to fixed lengths allows steel production and user departments to effectively save metal, facilitate production organization, fully utilize equipment capacity, simplify packaging, and facilitate transportation. If some products exceed the fixed length, they are cut off online, and then the rolling mill directly produces 120mm round bars (round steel with a diameter of 120mm), with a yield typically reaching 88%. After producing YLG steel ingots of a certain grade using a 6t rectangular ingot mold and 3t YLG steel ingots, the ends were sawn off, and samples were taken for inclusion rating. The inclusion level of the YLG steel ingot produced by the 6t rectangular ingot mold was ≤1.5, comparable to the 3t ingot, while its yield was significantly improved.
[0051] 4. The final raw steel produced after rolling and sawing of 4.6t rectangular raw steel ingots is φ120mm in diameter and 190~240mm in length (e.g., Figure 10 The specifications and length of the raw steel produced by the conventional 3t steel ingot process are consistent.
[0052] The innovative points of this invention are summarized as follows: (1) An innovative heating process was developed for a certain grade of raw steel ingot before rolling, which released the heat-releasing capacity of the rolling mill.
[0053] The 6t raw steel ingot mold has a rectangular cross-sectional shape. Compared with the traditional 3t square steel ingot mold, the 6t raw steel ingot mold provided by this invention has a smaller ingot body taper and a larger height-to-diameter ratio. The shape of the 6t raw steel is closer to that of a square continuously cast billet (as shown in Table 4, which is a comparison table of the shape parameters of the 6t rectangular steel ingot mold and the 3t square steel ingot mold). The subsequent rolling process does not require heating in the soaking pit (process flow is as follows). Figure 11 (As shown). The 6t raw steel ingot is heated in a continuous heating furnace and then finally rolled into round steel products. Compared with the 3t steel ingot forming process, the heating process in a soaking furnace is avoided.
[0054] Table 4 (2) The molten steel has a short solidification time in the mold, and the molten steel is not prone to component segregation in the solidification direction. The carbon and sulfur content of the steel ingot can meet the standard requirements.
[0055] Although the 6t rectangular steel ingot mold provided by this invention is relatively long, the casting time of the ingot body is the same as that of the 3t square ingot. The solidification time of molten steel in the ingot mold mainly depends on the radius of the ingot mold. The large and small end specifications of the 6t raw material steel ingot mold are both smaller than those of the 3t square steel ingot mold (as shown in Table 5, which is a comparison of the large and small end dimensions of the 6t raw material steel ingot mold and the traditional 3t square steel ingot mold). The solidification time of molten steel in the 6t rectangular steel ingot mold is shorter than that in the 3t square steel ingot mold. Compared with the 3t square steel ingot mold, the molten steel solidifies faster in the 6t rectangular steel ingot mold. When the molten steel solidifies in the mold, it is less prone to component segregation in the solidification direction. The chemical composition of both the large and small ends of the final formed steel ingot meets the requirements of Table 2.
[0056] Table 5 (3) The yield rate has been improved compared with the original process.
[0057] The 6t rectangular steel ingot has a slender shape and a filler ratio of 9% (calculated as shown in Table 6, which lists the specific dimensions of the 6t rectangular steel ingot in this invention). This filler ratio is only half that of the 18% filler ratio of the 3t square steel ingot. The 6t rectangular steel ingot also has a higher yield. The yield of the 6t rectangular raw material steel ingot is 88%, a significant improvement compared to the 80.5% yield of the 3t square raw material steel ingot.
[0058] Table 6 The specific implementation process of this invention is as follows: (1) Casting method: bottom pouring casting.
[0059] The 6t rectangular steel ingot mold is cast using the bottom pouring method, with three steel ingot molds placed on one tray during mold placement.
[0060] (2) Equipment or apparatus or component.
[0061] a) Insulation plate. Before the 6t rectangular steel ingot mold is set up, a split insulation plate with matching dimensions needs to be installed inside the riser of the steel ingot mold.
[0062] b) Base plate. The base plate is a disc-shaped casting component with a vertical riser hole in the center. The bottom of the 6t rectangular steel ingot mold is hollow, and the 6t rectangular steel ingot mold needs to be placed vertically on the base plate when it is being cast. During casting, molten steel flows into the steel ingot mold from the riser hole in the base plate.
[0063] c) Inlet Pour Pipe. Since the 6t rectangular steel ingot mold is 5m high, which is quite large, and a base plate is needed under the ingot mold during casting, multiple bases (serving the same purpose as the base plate) are placed under the inlet pour pipe during actual mold placement to ensure sufficient static pressure of the molten steel during casting and to ensure the 6t special rectangular mold is filled.
[0064] d) Base Plate. Before pouring steel, direct current bricks need to be laid in the grooves of the base plate. There are three grooves on the base plate that need direct current bricks, and a center brick needs to be laid in the central recess of the base plate. During pouring, the ladle outlet faces the opening of the central inlet pipe. After the ladle nozzle is opened, the molten steel flows down along the inner cavity of the central inlet pipe, into the inner cavity of the center brick of the base plate, and then continues to flow horizontally into the inner channels of the three direct current bricks until it reaches the tail brick and rises vertically into the riser hole of the base plate. Molten steel continuously flows into the ingot mold until it is completely filled.
[0065] This invention provides a method for casting a 6t rectangular steel ingot. The method includes: Step 1, setting up a 6t rectangular steel ingot mold, wherein the casting cavity of the 6t rectangular steel ingot mold is a rectangular, necked, and elongated cavity structure, the casting cavity of the 6t rectangular steel ingot mold is elongated to not less than 5000mm, at least one pair of side dimensions in the cross-section of the casting cavity of the 6t rectangular steel ingot mold are reduced, and the height-to-diameter ratio of the casting cavity of the 6t rectangular steel ingot mold is in the range of 9.5-10.0; Step 2, installing the 6t rectangular steel ingot mold and pouring molten steel into the casting cavity of the 6t rectangular steel ingot mold using a pit casting method; Step 3, demolding the steel ingot from the 6t rectangular steel ingot mold, then heating and cutting the billet.
[0066] Through the above-described design, the 6t rectangular steel ingot casting method provided by this invention has at least the following beneficial effects: In the 6t raw material steel ingot mold used in this invention, the cross-sectional size of the casting cavity is reduced, and the length of the casting cavity is increased. Compared with the 3t square steel ingot mold, the molten steel solidifies faster in the 6t rectangular steel ingot mold. During solidification in the mold, the molten steel is less prone to component segregation in the solidification direction. Due to the shortened solidification time in the casting cavity, the carbon and sulfur content of the steel ingot meets the standard requirements. Furthermore, because this invention increases the length of the casting cavity, the 6t rectangular raw material steel ingot cast by the 6t rectangular steel ingot mold provided by this invention, although a steel ingot, is relatively long. Therefore, it does not require heating in a soaking pit before rolling, but is heated in a continuous heating furnace in the steel rolling mill before subsequent processing. This effectively utilizes the capacity of the soaking pit in the steel rolling mill. Finally, the present invention saws off the ends of YLG steel ingots of a certain grade produced by a 6t rectangular steel ingot mold and 3t YLG steel ingots after they are finished, and samples are taken for inclusion rating. The inclusion level of the YLG steel ingot of a certain grade produced by the 6t rectangular steel ingot mold is ≤1.5 after it is finished, which is comparable to that of the 3t steel ingot. At the same time, its yield is significantly improved.
[0067] The above are merely preferred embodiments of the present invention and are not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for casting a 6t rectangular steel ingot, characterized in that, include: Step 1: Set up a 6t rectangular steel ingot mold for later use. The 6t rectangular steel ingot mold has a casting cavity and a riser structure. The cross-section of the casting cavity is rectangular. The cross-sectional dimensions of the upper end of the casting cavity are 500 mm × 380 mm, and the cross-sectional dimensions of the lower end of the casting cavity are 460 mm × 340 mm, thus making the entire casting cavity a conical structure. The height of the casting cavity is 4630 mm. The riser structure is connected to the casting cavity and forms a stepped opening structure with an enlarged opening at the top of the casting cavity. The height of the riser structure is 370 mm, and the cross-sectional dimensions of the riser structure are 540 mm × 420 mm. Step 2: Install the 6t rectangular steel ingot mold and pour molten steel into the casting cavity of the 6t rectangular steel ingot mold using the pit casting method; Step 3: Demold the steel ingot from the 6t rectangular steel ingot mold, then heat and open the billet.
2. The method for casting a 6t rectangular steel ingot according to claim 1, characterized in that, In step two, after fixing the 6t rectangular steel ingot mold, protective slag is set in the casting cavity of the 6t rectangular steel ingot mold by hanging method; Protective slag is placed in the casting cavity at positions 200mm±20mm from the bottom of the mold and at positions 500mm±50mm from the bottom of the mold. The amount of protective slag used is 2 kg / t.
3. The method for casting a 6t rectangular steel ingot according to claim 1, characterized in that, In step two, when fixing the 6t rectangular steel ingot mold, three 6t rectangular steel ingot molds are set on each base plate; The 6t rectangular steel ingot mold is mounted on the base plate via a chassis.
4. The method for casting a 6t rectangular steel ingot according to claim 1, characterized in that, In step two, during the process of pouring molten steel into the casting cavity of the 6t rectangular steel ingot mold, the casting time of the ingot body is 550-650 seconds, and the casting time of the riser is 180-300 seconds.
5. The method for casting a 6t rectangular steel ingot according to claim 1, characterized in that, The steel ingots are heated in a continuous heating furnace and then precision rolled into round steel products after being opened.
6. The method for casting a 6t rectangular steel ingot according to any one of claims 1 to 5, characterized in that, In step two, a central injection pipe is installed on the base plate, and molten steel is poured through the central injection pipe using a bottom injection method. The central injection tube is mounted on the base plate with adjustable height via a base; Multiple 6t rectangular steel ingot molds are arranged at equal intervals around the central injection pipe.
7. The method for casting a 6t rectangular steel ingot according to claim 6, characterized in that, The top of the injection tube is higher than the top of the 6t rectangular steel ingot mold, and the difference in height is N. The N is 8%-12% of the length of the 6t rectangular steel ingot mold.
Citation Information
Patent Citations
Method for manufacturing low segregation large-scale steel ingot
CN101234412A
Method for forging superhigh-temperature soft core of steel ingot
CN105268884A