Method for repairing surface defects of magnesium alloy components by laser cladding

By spraying a zinc shielding layer onto the surface of magnesium alloy components and using aluminum alloy powder for laser cladding repair, the safety risks of magnesium powder and the problem of magnesium-aluminum compounds hindering metallurgical bonding are solved, achieving efficient repair results and lightweight components.

CN118308719BActive Publication Date: 2026-11-24CHONGQING UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410427770.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-10
Publication Date
2026-11-24
Estimated Expiration
2044-04-10

AI Technical Summary

Technical Problem

Existing laser cladding technology poses safety risks when using magnesium powder to repair magnesium alloy components, and the formation of magnesium-aluminum compounds in the repair area severely hinders the metallurgical bonding effect.

Method used

After spraying a zinc shielding layer onto the surface of the magnesium alloy component, aluminum alloy powder is used for laser cladding repair to form a diffusion layer to reduce the magnesium-aluminum reaction. Specific laser power and process parameters are used to ensure that the aluminum and magnesium are fully melted and solidified rapidly.

Benefits of technology

It reduces the formation of magnesium-aluminum compounds, improves the metallurgical bonding between the repair layer and the substrate, ensures the repair effect while avoiding the safety risks of magnesium powder, and maintains the lightweight performance of the component.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118308719B_ABST
    Figure CN118308719B_ABST
Patent Text Reader

Abstract

This invention relates to a laser cladding repair method for surface defects in magnesium alloy components, belonging to the technical field of metal surface repair methods. The method includes the following steps: S1, spraying zinc onto the surface area of ​​the component to be repaired; S2, using aluminum alloy powder as raw material, using laser cladding technology to repair the zinc-sprayed surface area of ​​the component to be repaired. This invention uses aluminum alloy powder for laser cladding repair of magnesium alloy engineering components. Aluminum alloy powder is cheaper and safer than magnesium alloy powder. Furthermore, aluminum is a common alloying element in magnesium alloys, and using aluminum alloy to repair magnesium alloys does not incur additional costs for the subsequent recycling, refining, and reprocessing of the magnesium alloy components. Before laser cladding, zinc is sprayed as a shielding layer. During the repair process, a small amount of zinc diffuses with the magnesium and aluminum on both sides to form a solid solution diffusion layer, which greatly reduces the direct reaction between magnesium and aluminum, thereby reducing the amount of magnesium-aluminum compounds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of metal surface repair methods, and relates to a laser cladding repair method for surface defects of magnesium alloy components. Background Technology

[0002] Magnesium alloys are the lightest metallic structural materials, and magnesium alloy engineering components have broad application prospects in fields such as automotive lightweighting and aerospace. During application, magnesium alloy engineering components suffer structural damage due to wear and corrosion, which compromises their appearance and functionality. Directly replacing surface-damaged components not only incurs significant economic losses and resource waste but also fails to meet the requirements of comprehensively improving green manufacturing development. Therefore, employing appropriate remanufacturing technologies to repair damaged magnesium alloy components and restore their dimensions and function has significant economic and social benefits.

[0003] Laser cladding is a remanufacturing technology that uses a high-energy laser beam to simultaneously melt and rapidly solidify metal powder and a substrate, forming a metallurgically bonded cladding layer on the substrate surface. This technology is particularly suitable for processing high-performance coatings and remanufacturing on substrate surfaces. Laser cladding typically uses metal powder as a raw material. While magnesium powder has certain advantages as a material for repairing magnesium alloys, its reactive chemical properties make it highly flammable and explosive when exposed to water, moisture, or heat, and difficult to extinguish once ignited. Therefore, the use, storage, and transportation of magnesium powder pose significant risks. Considering that aluminum and magnesium have similar properties and melting points, and aluminum is safer than magnesium powder, and aluminum alloys undergo self-passivation in air, most aluminum alloys do not require additional surface treatment. Therefore, developing a technology using aluminum alloy powder to repair magnesium alloy components not only avoids the risks associated with using magnesium powder, but also ensures that the repaired components require little or no surface treatment.

[0004] Because laser cladding repair technology uses a high-energy laser beam as a heat source, the repair material and the substrate need to be melted simultaneously. Magnesium and aluminum are both reactive metals, and the maximum solid solubility of aluminum in magnesium is about 14%. During the solidification process in the repair area, aluminum and magnesium react with each other to produce Mg. 17 A l2 Compounds with high hardness will severely hinder the metallurgical bonding effect between the repair layer and the substrate.

[0005] Based on this, the present invention designs a method for repairing surface defects of magnesium alloy components using aluminum alloy powder, so as to reduce the formation of high-hardness metal compounds in the magnesium-aluminum repair area and ensure the repair effect. Summary of the Invention

[0006] In view of this, the purpose of the present invention is to provide a laser cladding repair method for surface defects of magnesium alloy components, so as to reduce the formation of high-hardness metal compounds in the magnesium-aluminum repair area and ensure the metallurgical bonding effect between the repair layer and the substrate.

[0007] To achieve the above objectives, the present invention provides the following technical solution: a method for laser cladding repair of surface defects in magnesium alloy components, comprising the following steps:

[0008] S1 applies zinc spraying to the surface area of ​​the component to be repaired to form a zinc shielding layer;

[0009] S2 uses aluminum alloy powder as raw material and laser cladding technology to repair the zinc shielding layer area, forming a repair layer. This repair layer contains a diffusion layer, which is a solid solution formed by the interdiffusion of zinc diffused from within the zinc shielding layer to the outside, and magnesium and aluminum on both sides.

[0010] Optionally, before step S1, the method further includes:

[0011] Step S0 involves pre-treating the surface area of ​​the component to be repaired, exposing the magnesium alloy surface.

[0012] Optionally, in step S0, the pretreatment may be carried out by sandblasting or surface mechanical grinding.

[0013] Optionally, after step S2, the following steps are also included:

[0014] Step S3 removes excess material from the surface of the repair layer area to restore the original dimensions of the component.

[0015] Optionally, in step S1, the thickness of the zinc shielding layer is 3%-8% of the thickness of the area to be repaired.

[0016] Optionally, the thickness of the zinc shielding layer is preferably 5% of the thickness of the area to be repaired.

[0017] Optionally, in step S2, the aluminum alloy powder is Al10Si7Mg powder, which is spherical powder with a particle size of 300 mesh.

[0018] Optionally, in step S2, the laser cladding repair process parameters are: spot size 3mm, laser power 750W-1500W, scanning speed 33.3mm / s-66.6mm / s, powder feeding speed 3.6g / min-6g / min; at this time, the linear energy density is 20-40J / mm, and the linear powder density is 0.001-0.0015g / mm.

[0019] Optionally, in step S2, the laser cladding repair process parameters are preferably: spot size 3mm, laser power 1000W, scanning speed 44.4mm / s, and powder feeding speed 3.6g / min; at this time, the linear energy density is 22.52J / mm and the linear powder density is 0.0013g / mm. Optionally, the diffusion layer thickness is 20-50μm, and there are no blocky magnesium-aluminum compounds near the diffusion layer.

[0020] The beneficial effects of this invention are as follows:

[0021] 1. This invention uses aluminum alloy powder for laser cladding repair of magnesium alloy engineering components. Aluminum alloy powder is cheaper and safer than magnesium alloy powder, making its use in place of magnesium alloy powder a significant engineering application. Furthermore, aluminum is a common alloying element in magnesium alloys, so using aluminum alloy to repair magnesium alloy components will not incur additional costs for subsequent recycling, refining, or reprocessing. In addition, aluminum alloy and magnesium alloy have similar densities and mechanical properties, so using aluminum alloy to repair magnesium alloy components will not affect the lightweight effect of the components.

[0022] 2. In this invention, zinc is sprayed as a shielding layer before laser cladding. During the repair process, a small amount of zinc diffuses with magnesium and aluminum on both sides to form a solid solution diffusion layer. Through the transition between magnesium and aluminum by zinc, the direct reaction between magnesium and aluminum is greatly reduced, thereby reducing the amount of magnesium-aluminum compounds and avoiding matrix embrittlement and cracking caused by magnesium-aluminum compounds, thus improving the bonding effect between the repair layer and the matrix.

[0023] 3. This invention uses a specific range of laser power and process parameters to ensure that aluminum and magnesium are fully melted, while rapid scanning ensures that the repair area solidifies quickly, reducing the generation of magnesium-aluminum compounds and improving the metallurgical bonding effect.

[0024] Other advantages, objectives, and features of the invention will be set forth in part in the description which follows, and in part will be apparent to those skilled in the art from the following examination, or may be learned from practice of the invention. The objectives and other advantages of the invention can be realized and obtained through the following description. Attached Figure Description

[0025] To make the objectives, technical solutions, and advantages of the present invention clearer, the preferred embodiments of the present invention will be described in detail below with reference to the accompanying drawings, wherein:

[0026] Figure 1 This is a schematic diagram of the repair method of the present invention;

[0027] Figure 2 Microscopic tissue photographs of the repaired area in Example 1;

[0028] Figure 3Microscopic images of the repaired area in Example 2;

[0029] Figure 4 Microscopic images of the repaired area in Example 3;

[0030] Figure 5 Microscopic tissue photographs of the repaired area in Example 4;

[0031] Figure 6 Here is a macroscopic photograph of the sample after repair in Example 1;

[0032] Figure 7 This is a macroscopic photograph of the sample after repair in Example 2;

[0033] Figure 8 Here is a macroscopic photograph of the sample after repair in Example 3;

[0034] Figure 9 This is a macroscopic photograph of the sample after repair in Example 4. Detailed Implementation

[0035] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the illustrations provided in the following embodiments are only schematic representations of the basic concept of the present invention. Unless otherwise specified, the following embodiments and features can be combined with each other.

[0036] The accompanying drawings are for illustrative purposes only and are schematic diagrams, not actual pictures. They should not be construed as limiting the invention. To better illustrate the embodiments of the invention, some parts in the drawings may be omitted, enlarged, or reduced, and do not represent the actual product dimensions. It is understandable to those skilled in the art that some well-known structures and their descriptions may be omitted in the drawings.

[0037] In the accompanying drawings of the embodiments of the present invention, the same or similar reference numerals correspond to the same or similar components. In the description of the present invention, it should be understood that if terms such as "upper," "lower," "left," "right," "front," and "rear" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the drawings, they are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, the terms used to describe positional relationships in the drawings are only for illustrative purposes and should not be construed as limiting the present invention. For those skilled in the art, the specific meaning of the above terms can be understood according to the specific circumstances.

[0038] Example 1

[0039] In this embodiment, AZ31 magnesium alloy is used as the repair object. A 5mm thick AZ31 magnesium alloy plate is taken, and a notch with a depth of 1mm and a width of 2mm is first cut on the surface of the magnesium alloy plate using a grinding wheel. Then, the notch is repaired using the method of this embodiment, and the repair effect is recorded.

[0040] Please see Figures 1-9 This is a laser cladding repair method for surface defects in magnesium alloy components, such as... Figure 1 As shown, it includes the following steps:

[0041] S0 involves sandblasting the surface area of ​​the component to be repaired to remove oxides, impurities, etc., exposing the magnesium alloy surface; pretreatment can be carried out by various methods such as sandblasting and surface mechanical grinding.

[0042] S1 sprays zinc onto the surface area of ​​the component to be repaired, i.e., the exposed magnesium alloy surface, to form a zinc shielding layer with a thickness of 5% of the thickness of the area to be repaired.

[0043] S2 uses aluminum alloy powder as raw material and laser cladding technology to repair the zinc shielding layer area to form a repair layer. The repair material used in laser cladding is Al10Si7Mg powder, which is spherical powder with a particle size of 300 mesh. The laser cladding repair process parameters are: spot size 3mm, laser power 750W, scanning speed 33.3mm / s, and powder feeding speed 3.6g / min.

[0044] S3: Use grinding to remove excess material from the surface of the repair layer area from step S2, restoring the original dimensions of the component. Other post-processing methods, such as milling, can also be used.

[0045] In this embodiment, due to the relatively low laser power of 750W, the cladding speed of the substrate and the repair material is slow, the mutual diffusion of aluminum and magnesium atoms is restricted, the repair material fails to fully fill the gap, and the repair effect is not ideal.

[0046] Example 2

[0047] The difference from Example 1 is as follows:

[0048] In step S2, the laser cladding repair process parameters are: spot size 3mm, laser power 1500W, scanning speed 33.3mm / s, and powder feeding speed 3.6g / min.

[0049] In this embodiment, the laser power is increased to 1500W. At this point, the temperature of the molten pool is high, which easily produces defects such as pores, resulting in an unsatisfactory repair effect.

[0050] Example 3

[0051] The difference from Example 1 is as follows:

[0052] In step S1, in this embodiment, zinc spraying was not applied to the surface area of ​​the component to be repaired, and the zinc spraying layer was not used as a shielding layer for subsequent laser cladding repair, as a comparison.

[0053] In step S2, the laser cladding repair process parameters are: spot size 3mm, laser power 1000W, scanning speed 44.4mm / s, and powder feeding speed 3.6g / min.

[0054] In this embodiment, since magnesium and aluminum can only be partially miscible and magnesium atoms have relatively small radii, magnesium atoms tend to diffuse into aluminum during laser cladding repair. During solidification, magnesium and aluminum react with each other to form a eutectic phase or metal compound. The brittle eutectic phase and metal compound affect the metallurgical bonding of the repair interface, leading to defects or even detachment in the repair area. Therefore, a shielding layer needs to be added during laser cladding to hinder the direct reaction between magnesium and aluminum during laser repair to reduce the formation of high-hardness magnesium-aluminum compounds.

[0055] Example 4

[0056] The difference from Example 1 is as follows:

[0057] In step S2, aluminum alloy powder is used as raw material, and laser cladding technology is used to repair the zinc shielding layer area to form a repair layer. The repair layer contains a diffusion layer, which is a dark diffusion layer with a thickness of 20-50μm, and there are no large blocks of high-hardness magnesium-aluminum compounds near the diffusion layer. The laser cladding repair process parameters are: spot size 3mm, laser power 1000W, scanning speed 44.4mm / s, and powder feeding speed 3.6g / min.

[0058] like Figure 2 As shown, this is a schematic diagram of the microstructure after repair in Example 1. Figure 2 As can be seen, due to the insufficient laser power of 750W, the repair material failed to fully fill the gap, resulting in a less than ideal repair effect; for example... Figure 3 As shown, this is a schematic diagram of the microstructure after repair in Example 2. Figure 3 As can be seen, a laser power of 1500W is too high. At this power, the high temperature of the molten pool easily leads to defects such as porosity, resulting in a less than ideal repair effect. For example... Figure 4 As shown, Figure 4 For example, a tissue micrograph of the repaired tissue in Example 3, from Figure 4 It can be seen that there are a large number of black compounds and cracks at the interface between the substrate and the repair material. The black compounds are formed due to the interdiffusion of magnesium and aluminum, which reacts during the solidification process, producing Mg17 Al l2 High-hardness compounds severely hinder the metallurgical bonding effect between the repair layer and the substrate, reducing the interfacial bonding force. Therefore, the addition of a shielding layer is essential.

[0059] Because laser cladding repair involves melting magnesium and aluminum with a high-energy beam before solidification, excessive energy input during solidification not only produces more magnesium-aluminum compounds but also results in an excessively large heat-affected zone, causing thermal shrinkage and affecting the component's dimensions. Conversely, low energy input prevents alloying elements from effectively forming a metallurgical bond, hindering effective repair. Therefore, in step S2, the laser cladding repair process parameters are: spot size 3mm, laser power 750W-1500W, scanning speed 33.3mm / s-66.6mm / s, and powder feeding speed 3.6g / min-6g / min. At this range, the linear energy density is 20-40J / mm², and the linear powder density is 0.0001-0.0015g / mm². This range of linear energy density and linear powder density ensures that the Al10Si7Mg powder is relatively uniformly distributed in the molten pool under the action of the laser beam, forming a high-quality cladding layer.

[0060] Example 4 is a preferred embodiment of the present invention, wherein the thickness of the zinc shielding layer is preferably 5% of the thickness of the area to be repaired, and the laser cladding repair process parameters are preferably: spot size 3mm, laser power 1000W, scanning speed 44.4mm / s, powder feeding speed 3.6g / min; at this time, the linear energy density is 22.52J / mm, and the linear powder density is 0.0013g / mm. Figure 5 The image shows a microscopic tissue photograph of Example 4. It can be seen from the image that there is a dark diffusion layer with a thickness of 20-50 μm at the interface of the repair layer, and there are no large blocks of high-hardness magnesium-aluminum compounds near the diffusion layer. This indicates that the addition of the zinc shielding layer and appropriate laser process parameters have a positive effect on the interdiffusion of magnesium and aluminum in the tissue.

[0061] Figures 6-9 These are macroscopic photographs of the samples after repair in Examples 1 to 4. In Example 1, some repair gaps still exist, and the repair material failed to fully fill the gaps. In Example 2, due to excessively high laser power, metal evaporation occurred during the repair process, resulting in macroscopic defects in the repair area. In Example 3, the repair area appears to be of good quality macroscopically, but microscopic analysis reveals numerous compounds at the repair interface, such as... Figure 4 Example 4 showed no visual difference and achieved a good repair effect.

[0062] In this embodiment of the invention, Al is used. 10Using Si7Mg aluminum alloy powder to repair AZ31 magnesium alloy components is feasible because the melting points of magnesium and aluminum are not much different. Aluminum alloys and magnesium alloys have similar densities and mechanical properties, so using aluminum alloy materials to repair magnesium alloy components will not affect the lightweight effect of the components. At the same time, aluminum alloy is a common alloying element in magnesium alloys, so using aluminum alloy to repair magnesium alloy will not bring additional costs to the subsequent recycling, refining and reprocessing of magnesium alloy components.

[0063] Compared with Embodiment 3 of the present invention, in Embodiments 1, 2, and 4 of the present invention, zinc is sprayed as a shielding layer before laser cladding. During the laser cladding repair process, magnesium atoms diffuse into zinc to form a solid solution, and aluminum atoms diffuse into the zinc shielding layer to form a solid solution. The strength of zinc is lower than that of aluminum and magnesium. A small amount of zinc diffuses with magnesium and aluminum on both sides to form a solid solution diffusion layer, which greatly reduces the direct reaction between magnesium and aluminum. Since the strength of zinc is lower than that of aluminum and magnesium, an excessively thick zinc shielding layer will affect the strength of the transition zone, while an excessively thin shielding layer will result in an insignificant shielding effect. The thickness of the zinc shielding layer is 3%-8% of the thickness of the repair zone. A small amount of zinc diffuses with magnesium and aluminum on both sides to form a solid solution diffusion layer, which greatly reduces the direct reaction between magnesium and aluminum and reduces the amount of magnesium-aluminum compounds; thereby reducing the amount of magnesium-aluminum compounds.

[0064] In this embodiment of the invention, laser cladding repair involves melting magnesium and aluminum with a high-energy beam input before solidification. Excessive energy input during solidification not only produces more magnesium-aluminum compounds but also results in an excessively large heat-affected zone, causing thermal shrinkage and affecting the component's dimensions. Conversely, low energy input prevents the effective formation of metallurgical bonds between alloying elements, hindering effective repair. Therefore, in the preferred embodiment 4 of this invention, a moderate laser power is used accompanied by rapid scanning. The process window is a linear energy density of 20-40 J / mm² and a linear powder density of 0.0001-0.0015 g / mm². The moderate laser power ensures the melting of magnesium and aluminum, while the rapid scanning ensures rapid solidification of the repair area, avoiding the formation of magnesium-aluminum compounds.

[0065] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.

Claims

1. A method for repairing surface defects of a magnesium alloy member by laser cladding, characterized by, Includes the following steps: S1. Spray zinc onto the surface area of ​​the component to be repaired to form a zinc shielding layer, the thickness of which is 3%-8% of the thickness of the area to be repaired; S2 uses aluminum alloy powder as raw material and laser cladding technology to repair the zinc shielding layer area to form a repair layer. The aluminum alloy powder is Al10Si7Mg powder, which is spherical powder with a particle size of 300 mesh. The laser cladding repair process parameters are: spot size 3mm, laser power 750W-1500W, scanning speed 33.3mm / s-66.6mm / s, powder feeding speed 3.6g / min-6g / min; at this time, the linear energy density is 20-40J / mm, and the linear powder density is 0.001-0.0015g / mm. The repair layer contains a diffusion layer, which is formed by the diffusion of zinc from the zinc shielding layer to the outside with the mutual diffusion of magnesium and aluminum on both sides to form a solid solution. The thickness of the diffusion layer is 20-50μm, and there are no blocky magnesium-aluminum compounds near the diffusion layer.

2. The method of claim 1, wherein Before step S1, the following is also included: Step S0 involves pre-treating the surface area of ​​the component to be repaired, exposing the magnesium alloy surface.

3. The method of claim 2, wherein the magnesium alloy member surface defect laser cladding repair method is characterized by, In step S0, the pretreatment is carried out by sandblasting or surface mechanical grinding.

4. The method of claim 1, wherein Following step S2, the following is also included: Step S3 removes excess material from the surface of the repair layer area to restore the original dimensions of the component.

5. The method of claim 1, wherein The thickness of the zinc shielding layer is preferably 5% of the thickness of the area to be repaired.

6. The method of claim 1, wherein In step S2, the preferred laser cladding repair process parameters are: spot size 3mm, laser power 1000W, scanning speed 44.4mm / s, and powder feeding speed 3.6g / min; at this time, the linear energy density is 22.52J / mm and the linear powder density is 0.0013g / mm.