PMMA composite material, preparation method and application thereof
By incorporating core-shell structured acrylate rubber and ethylene bis-stearamide into PMMA material, the problems of easy cracking and insufficient scratch resistance of PMMA material after injection molding are solved, achieving high hardness and scratch resistance, while avoiding material defects.
Patent Information
- Application Number
- CN202410538666.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-30
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-04-30
AI Technical Summary
PMMA material is prone to cracking after injection molding, and it is difficult to balance scratch resistance and hardness. In addition, material defects are prone to occur when injection molding complex structural parts.
A core-shell structured acrylate rubber and ethylene bis-stearamide were used as modifiers to control the core particle size within the range of 180–250 nm. 2–5% ethylene bis-stearamide was added to PMMA resin, and PMMA composite materials were prepared by melt extrusion.
It improves the stress cracking resistance, hardness, and scratch resistance of PMMA composite materials, and avoids material sputtering problems when injection molding complex structural parts.
Smart Images

Figure BDA0004820416490000071 
Figure BDA0004820416490000072 
Figure BDA0004820416490000081
Abstract
Description
Technical Field
[0001] This invention relates to the field of engineering plastics technology, and more specifically, to a PMMA composite material, its preparation method, and its application. Background Technology
[0002] Polymethyl methacrylate (PMMA) resin has high scratch resistance and weather resistance, and can be widely used in the exterior decoration parts of windows and pillars of products such as household appliances and automobiles. However, PMMA material has high internal stress, and it is prone to cracking after injection molding due to high internal stress, which limits its application in the automotive and household appliance fields.
[0003] Existing technologies address the issue of PMMA materials being prone to cracking due to high stress by adding toughening agents (such as butadiene rubber toughening agents MBS, SBC rubber, and ABS high-rubber powder). However, the addition of these toughening agents can easily reduce the material's scratch resistance and hardness, potentially limiting its application in certain scenarios, such as smart home applications where better scratch resistance and hardness are required.
[0004] Furthermore, with the increasing demands for lightweight and intelligent design in automobiles and home appliances, the structures of product components are becoming more complex. For example, the large air inlet and outlet grilles of air purifiers have narrow flow channels and strong shearing, making it difficult to exhaust air and causing the components to easily develop undesirable appearance defects such as material defects.
[0005] Therefore, new technologies need to be developed to solve the technical problems of PMMA materials not being able to simultaneously achieve stress cracking resistance, scratch resistance and hardness, as well as the appearance defects of material spots that easily appear after injection molding into complex structural parts. Summary of the Invention
[0006] The primary objective of this invention is to overcome the current problems of PMMA materials not being able to simultaneously achieve resistance to stress cracking, scratch resistance, and hardness, as well as the tendency for material defects to appear after injection molding into complex structural parts, and to provide a PMMA composite material.
[0007] A further object of the present invention is to provide a method for preparing the above-mentioned PMMA composite material.
[0008] A further object of the present invention is to provide the application of the above-mentioned PMMA composite material in the manufacture of smart home appliances or automotive parts.
[0009] The above-mentioned objective of the present invention is achieved through the following technical solution:
[0010] A PMMA composite material comprises the following components in parts by weight:
[0011] 100 parts PMMA resin
[0012] 5-11 parts of acrylate rubber,
[0013] 2-5 parts of ethylene bis-stearamide;
[0014] The acrylate rubber has a core-shell structure, with the core having an average particle size of 180–250 nm (specifically, 180 nm, 185 nm, 190 nm, 195 nm, 200 nm, 205 nm, 210 nm, 215 nm, 220 nm, 230 nm, 240 nm, or 250 nm), and the shell being polymethyl methacrylate.
[0015] The inventors of this invention discovered through research that by adding an acrylate rubber with a core-shell structure and a shell of polymethyl methacrylate to PMMA resin, while controlling the particle size of the core within a suitable range, the stress cracking resistance of PMMA composite materials can be improved to a certain extent, and the PMMA composite materials can also have higher hardness and scratch resistance.
[0016] Ethylene bis-stearamide is commonly added to PMMA resin materials as a lubricant, but its addition amount is usually less than 2% of the PMMA resin. The inventors of this invention have discovered that adding a higher amount of ethylene bis-stearamide (ethylene bis-stearamide at 2-5% of the PMMA resin by mass) not only improves the compatibility between PMMA resin and acrylic rubber, but also makes the molecular chains of PMMA resin more flexible. This further improves the stress cracking resistance of PMMA composite materials and effectively avoids material flow problems that occur when PMMA composite materials are injection molded into complex structural parts; simultaneously, it also helps the PMMA resin material maintain a high hardness.
[0017] The PMMA composite material of the present invention has high surface hardness, good scratch resistance and good stress cracking resistance, and can effectively avoid material sputtering problems that occur when injection molding complex structural parts.
[0018] In this invention, PMMA resin is used as the main resin, and it accounts for at least 80% of the mass of the PMMA composite material.
[0019] Optionally, the melt flow rate of the PMMA resin, measured at 230°C and 3.8 kg, is 1–15 g / 10 min. The melt flow rate of the PMMA resin can be measured according to ISO 1133-2022.
[0020] In this invention, the average particle size of the core of the acrylate rubber can be measured by a particle size analyzer.
[0021] The acrylate rubber of this invention can be commercially available (such as LG EM500 from South Korea) or can be manufactured in-house.
[0022] Typically, the ratio of the core diameter to the shell thickness of the acrylate rubber is (1-40):1.
[0023] The core of the acrylic rubber is a toughening component. The toughening component does not melt during the preparation process (melt extrusion) of the PMMA composite material. Therefore, as long as the average particle size of the core meets the requirements of this invention, there is no need to specifically limit the composition or structure of the core.
[0024] Preferably, the core of the acrylate rubber is a copolymer of methyl methacrylate-butyl acrylate-styrene or a copolymer of methyl methacrylate-butadiene-styrene.
[0025] More preferably, the core of the acrylate rubber is a copolymer of methyl methacrylate-butyl acrylate-styrene. When the core of the acrylate rubber is a copolymer of methyl methacrylate-butyl acrylate-styrene, the resulting PMMA composite material has higher surface hardness, better scratch resistance, and a better appearance when injection molded into complex structural parts.
[0026] More preferably, when the core of the acrylate rubber is a copolymer of methyl methacrylate-butyl acrylate-styrene, the acrylate rubber can be prepared by the following process: mixing methyl methacrylate monomer, a first emulsifier, a first initiator, and a solvent, and performing a first-stage emulsion polymerization (reacting at 70-75°C for 1.5-2.2 hours), then adding butyl acrylate, styrene, and a crosslinking agent, and performing a second-stage emulsion polymerization (reacting at 70-75°C for 1-2 hours) to obtain tough particles; mixing the tough particles with a second emulsifier, a second initiator, and a solvent, and reacting at 70-80°C for 1-3 hours to obtain the acrylate rubber.
[0027] The first emulsifier and the second emulsifier may be the same or different. Preferably, the first emulsifier and the second emulsifier independently include, but are not limited to, at least one of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, and potassium stearate.
[0028] The first initiator and the second initiator can be the same or different. Preferably, the first initiator and the second initiator independently include, but are not limited to, at least one of potassium persulfate, cumene peroxide, and dicumene peroxide.
[0029] More preferably, the solvent is water; the crosslinking agent is at least one of allyl methacrylate, ethylene glycol dimethacrylate, or trimethylolpropane trimethacrylate.
[0030] Preferably, the core particle size of the acrylate rubber is 180–200 nm. Within this particle size range, the resulting PMMA composite material has higher surface hardness and better scratch resistance.
[0031] Preferably, the ethylene bis-stearamide has a mass percentage of 3.5% to 5% relative to the PMMA resin. Within this mass percentage range, the resulting PMMA composite material exhibits better scratch resistance and stress cracking resistance.
[0032] The PMMA composite material of the present invention may also include 0.1 to 2 parts of other additives without affecting the effect of the present invention; the other additives include antioxidants, other lubricants, colorants, antistatic agents, etc., and the amount of each other additive can be: 0.1 to 0.5 parts of antioxidants, 0.1 to 2 parts of other lubricants, 0.1 to 1.5 parts of colorants, and 0.1 to 0.5 parts of antistatic agents.
[0033] Optionally, the antioxidant is a hindered phenolic antioxidant and / or a phosphite antioxidant.
[0034] Optionally, the hindered phenolic antioxidant is at least one of antioxidant 1076, antioxidant 1010, or antioxidant 259.
[0035] Optionally, the phosphite antioxidant is at least one of antioxidant 626, antioxidant 168, or antioxidant PEP 36.
[0036] Optionally, the other lubricants include, but are not limited to, at least one of oleamide or erucamide.
[0037] Optionally, the colorant includes, but is not limited to, at least one of titanium dioxide or carbon black.
[0038] Optionally, the antistatic agent includes, but is not limited to, at least one of polyether ester amide or polyether ester imide.
[0039] Preferably, the PMMA composite material further includes 1 to 3 parts of filler, wherein the filler includes, but is not limited to, at least one of barium sulfate, talc, or calcium carbonate.
[0040] The preparation method of the above-mentioned PMMA composite material includes the following steps: mixing the components, melt extruding, and granulating to obtain the PMMA composite material.
[0041] Preferably, the temperature of the melt extrusion is 120-240°C, the screw speed of the extruder is 300-500 rpm, and the length-to-diameter ratio of the screw is 40-65:1.
[0042] The application of the aforementioned PMMA composite material in the preparation of smart home appliance components or automotive components is also within the scope of protection of this invention.
[0043] The smart home appliance component is the grille of an air purifier.
[0044] Compared with the prior art, the beneficial effects of the present invention are:
[0045] The PMMA composite material of the present invention has high hardness, good scratch resistance and good stress cracking resistance, and can effectively avoid material sputtering problems that occur when injection molding complex structural parts. Detailed Implementation
[0046] To more clearly and completely describe the technical solution of the present invention, the present invention will be further described in detail below through specific embodiments. It should be understood that the specific embodiments described herein are only for explaining the present invention and are not intended to limit the present invention. Various changes can be made within the scope of the claims of the present invention.
[0047] The reagents used in the various embodiments and comparative examples of this invention are described below:
[0048] PMMA resin #1: Rohm, 7N;
[0049] PMMA resin #2: Rohm, 8N;
[0050] PMMA resin #3: Rohm, 6N;
[0051] Acrylic rubber #1: Core-shell structure, with the core being a copolymer of methyl methacrylate-butyl acrylate-styrene, and the shell being polymethyl methacrylate; self-made, the preparation process is as follows:
[0052] 1) Add appropriate amounts of deionized water, sodium dodecyl sulfate emulsifier, and potassium persulfate initiator to a 250 mL four-necked flask. Adjust the pH to 8.5 with dilute NaOH solution, purge with nitrogen, and stir for 20 min. Then add methyl methacrylate monomer, heat to 73 °C, and carry out the first stage of the reaction for 1.5 h. Then add a mixture of butyl acrylate, styrene, and allyl methacrylate crosslinking agent. After the addition is complete, carry out the second stage of the reaction at 73 °C for 1 h to obtain an emulsion containing P(BA-St) / PMMA tough particles. The particle size (i.e., the core particle size) of the P(BA-St) / PMMA tough particles was measured to be 180 nm by a particle size analyzer.
[0053] 2) Add a certain amount of deionized water, sodium dodecyl sulfate, potassium persulfate, and a calculated amount of PMMA / P(BA-St) toughening particles to a 2000mL four-necked flask. Purge with nitrogen, stir, and heat to 75℃. Begin adding methyl methacrylate monomer dropwise, completing the addition in about 3 hours, and maintain the temperature for 2 hours. Discharge and filter the material. Take an appropriate amount of the emulsion for testing, and freeze the remaining emulsion to break the emulsion. Filter and dry to obtain acrylic rubber #1.
[0054] Acrylic rubber 2#: Core-shell structure, the core is a copolymer of methyl methacrylate-butyl acrylate-styrene, the shell is polymethyl methacrylate, and the core particle size is 200nm; self-made, the preparation process is basically the same as that of acrylic rubber 1#, the difference is: in step 1), the heat preservation reaction time of the first stage is 1.8h (under the condition that other conditions remain unchanged, the particle size of the acrylic rubber core can be controlled by adjusting the heat preservation reaction time of the first stage).
[0055] Acrylic rubber 3#: core-shell structure, the core is a copolymer of methyl methacrylate-butyl acrylate-styrene, the shell is polymethyl methacrylate, and the particle size of the core is 220nm; self-made, the preparation process is basically the same as that of acrylic rubber 1#, the difference is that in step 1), the heat preservation reaction time of the first stage is 2.1h.
[0056] Acrylic rubber #4: EM500, LG Korea; core-shell structure, the core is a copolymer of methyl methacrylate-butadiene-styrene, the shell is polymethyl methacrylate, and the particle size of the core is 200nm.
[0057] Acrylic rubber 5#: core-shell structure, the core is a copolymer of methyl methacrylate-butyl acrylate-styrene, the shell is polymethyl methacrylate, and the particle size of the core is 150nm; self-made, the preparation process is basically the same as that of acrylic rubber 1#, the difference is that in step 1), the heat preservation reaction time of the first stage is 1h.
[0058] Acrylic rubber 6#: core-shell structure, the core is a copolymer of methyl methacrylate-butyl acrylate-styrene, the shell is polymethyl methacrylate, and the particle size of the core is 300nm; self-made, the preparation process is basically the same as that of acrylic rubber 1#, the difference is that in step 1), the heat preservation reaction time of the first stage is 3h.
[0059] Styrene-butadiene rubber: ASAFLEX 830, Asahi Kasei Corporation, Japan, styrene-butadiene block copolymer, rubber particle size is 200nm;
[0060] Ethylene bis-stearamide: Commercially available;
[0061] Pentaerythritol stearate: Commercially available;
[0062] Magnesium stearate: Commercially available;
[0063] Other additives #1: Antioxidant, which is obtained by mixing antioxidant 1010 and antioxidant 168 in a 1:1 mass ratio. Both antioxidant 1010 and antioxidant 168 are commercially available.
[0064] Unless otherwise specified, all components (e.g., other additives 1#) used in the parallel examples and comparative examples are the same commercially available products.
[0065] The luminescent PMMA composite materials of the embodiments and comparative examples of the present invention were prepared by the following preparation method:
[0066] Weigh each component according to the formula; mix the components, melt extrude in a twin-screw extruder, and granulate to obtain the PMMA composite material. The temperature of the twin-screw extruder is 120–190℃ in zones one and two, 200–240℃ in zones three and five, and 200–240℃ in zones five and ten. The screw speed is 400 rpm, and the screw length-to-diameter ratio is 52:1.
[0067] The performance of the PMMA composite materials provided in the embodiments and comparative examples of this invention was determined according to the following test methods:
[0068] (1) Surface hardness: Tested according to ISO 2039-2-2003 standard. A 12.7mm diameter ball indenter was used for the test. The test was conducted under a 10kg load for 1 minute. The scale was M scale.
[0069] (2) Scratch resistance: PMMA composite material was prepared into STUCCO textured plate samples inside KINGFA and tested according to Volkswagen's PV3952-2019-03 standard. Under a 10N load, the L value (L reflects the depth of color) at the same position before and after scratching was measured by a colorimeter. ΔL was calculated. The larger the ΔL value, the more obvious the whitening after scratching, and the worse the scratch resistance of the material.
[0070] (3) Stress cracking resistance: The tensile specimen with weld lines according to ISO 527-2-2012 standard was loaded into a fixture with a strain of 0.5%, and 1 ml of glacial acetic acid was added before the cracking time of the tensile specimen was calculated.
[0071] (4) Appearance of injection molding defects: The surface of the injection-molded gold-colored panel mold (mold structure reference CN102416690B) was observed to assess the severity of defects. The defect area was quantified as a percentage of the total panel area, where 0 indicates a smooth surface with no defects; 1 indicates slight defects; 2 indicates slight defects, accounting for <5% of the entire panel; 3 indicates a small amount of defects, accounting for 5-25% of the entire panel; 4 indicates a large amount of defects, accounting for 25-50% of the entire panel; and 5 indicates defects covering the entire panel.
[0072] Examples 1-11
[0073] Examples 1-11 provide a series of PMMA composite materials, the formulations of which are shown in Table 1.
[0074] Table 1. Formulations (parts by weight) for Examples 1-11
[0075]
[0076] Comparative Examples 1-9
[0077] Comparative Examples 1–9 provide a series of PMMA composite materials, the formulations of which are shown in Table 2.
[0078] Table 2 shows the formulations (parts by weight) for Comparative Examples 1–9.
[0079]
[0080] The properties of the PMMA composite materials of each embodiment and comparative example were determined according to the test methods mentioned above, and the test results are shown in Table 3.
[0081] Table 3 Performance test results of each embodiment and comparative example
[0082]
[0083] As can be seen from Table 3:
[0084] The PMMA composite materials in Examples 1-11 all have a surface hardness of over 82, a gloss difference of less than 1.4 in the scratch resistance test, a cracking time of more than 50 seconds in the stress cracking test, and an appearance grade of 0 or 1. This indicates that the PMMA composite material of the present invention has high hardness, good scratch resistance, and good stress cracking resistance, and can effectively avoid the material sputtering problem that occurs when injection molding complex structural parts.
[0085] In Comparative Examples 1 and 2, the particle size control of the acrylate rubber core was inappropriate. When the resulting PMMA composites were injection molded into complex structural parts, material sputtering was not significantly avoided. Furthermore, Comparative Example 1 exhibited poor stress cracking resistance, and Comparative Example 2 showed poor scratch resistance. In Comparative Example 3, the added rubber did not have a core-shell structure. The resulting PMMA composite had poor hardness, scratch resistance, and stress cracking resistance, and material sputtering was not significantly avoided when injection molded into complex structural parts. Comparative Example 4, without the addition of acrylate rubber, resulted in a PMMA composite with poor stress cracking resistance and severe material sputtering when injection molded into complex structural parts. In Comparative Examples 5 and 6, the added lubricant was inappropriate, resulting in PMMA composites with poor stress cracking resistance and material sputtering was not significantly avoided when injection molded into complex structural parts. In Comparative Example 7, the addition of too little ethylene bis-stearamide resulted in a PMMA composite with poor stress cracking resistance and material sputtering was not significantly avoided when injection molded into complex structural parts. In Comparative Example 8, too much ethylene bis-stearamide was added, resulting in poor hardness of the PMMA composite material. When injection-molded into complex structural parts, the problem of material speckling (surface precipitation) could not be significantly avoided. In Comparative Example 9, stearamide was added, resulting in PMMA composite material with poor stress cracking resistance. When injection-molded into complex structural parts, the problem of material speckling could not be significantly avoided.
[0086] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation of the present invention. Those skilled in the art can make other variations or modifications based on the above description. It is neither necessary nor possible to exhaustively describe all embodiments here. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the claims of the present invention.
Claims
1. A PMMA composite material, characterized in that, The components include the following parts by weight: 100 parts PMMA resin 5-10 parts of acrylate rubber, Ethylene bis-stearamide 2.5-5 parts; The acrylate rubber has a core-shell structure, with the core having an average particle size of 180~250nm and the shell being polymethyl methacrylate.
2. The PMMA composite material according to claim 1, characterized in that, The melt flow rate of the PMMA resin measured at 230℃ and 3.8kg was 1~15g / 10min.
3. The PMMA composite material according to claim 1, characterized in that, The core of the acrylate rubber is a copolymer of methyl methacrylate-butyl acrylate-styrene or a copolymer of methyl methacrylate-butadiene-styrene.
4. The PMMA composite material according to claim 3, characterized in that, The core of the acrylate rubber is a copolymer of methyl methacrylate-butyl acrylate-styrene.
5. The PMMA composite material according to claim 1, characterized in that, The core of the acrylate rubber has a particle size of 180~200nm.
6. The PMMA composite material according to claim 1, characterized in that, The ethylene bis-stearamide has a mass percentage of 3.5-5% relative to PMMA resin.
7. The PMMA composite material according to claim 1, characterized in that, The PMMA composite material includes 0.1 to 2 parts of other additives.
8. The PMMA composite material according to claim 7, characterized in that, The other additives are at least one of antioxidants, other lubricants, colorants, or antistatic agents.
9. A method for preparing the PMMA composite material according to any one of claims 1 to 8, characterized in that, The process includes the following steps: mixing the components, melt extrusion, and granulation to obtain the PMMA composite material.
10. The use of the PMMA composite material according to any one of claims 1 to 8 in the manufacture of smart home appliances or automotive parts.
Citation Information
Patent Citations
Mold for evaluating appearance of plastic
CN102416690B
Antiscratch resin and preparation method thereof
CN102190846A