Preparation method of super-hydrophilic antibacterial antireflection coating and antibacterial antireflection coating
By preparing antibacterial nanoparticles in situ on the surface of an inorganic nano-coating, a three-layer antireflective coating is formed, which solves the problems of easy microbial contamination and reduced light transmittance of the antireflective coating. It achieves a combination of high light transmittance and strong antibacterial properties, making it suitable for complex environments such as medical equipment.
Patent Information
- Application Number
- CN202410477124.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-19
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-04-19
AI Technical Summary
Existing anti-reflective coatings are easily contaminated by microorganisms in complex environments such as medical equipment, and the light transmittance is greatly reduced after the introduction of metal antibacterial agents, making it difficult to have both high anti-reflective ability and antibacterial performance.
Antibacterial nanoparticles were prepared on the surface of an inorganic nano-coating by in-situ reduction, forming a three-layer structure: the bottom layer is porous nano-silica or titanium dioxide, the middle layer is polydopamine, and the top layer is nano-silver particles, which improves the release efficiency of antibacterial agents at the interface and reduces light scattering.
The prepared coating has excellent anti-reflective properties and super antibacterial properties, with a light transmittance of up to 96%. It maintains a long-lasting antibacterial effect in humid environments, and the process is simple, environmentally friendly, and low in cost.
Smart Images

Figure CN118325367B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of anti-reflective coatings, and particularly relates to a method for preparing a superhydrophilic antibacterial and anti-reflective coating and the antibacterial and anti-reflective coating itself. Background Technology
[0002] Anti-reflective technology offers unique advantages in improving device transmittance, including high refractive index matching and wide applicability, particularly suitable for substrates with varying refractive indices within a system. In the field of optical coatings, porous inorganic nanoparticle anti-reflective coatings prepared via the sol-gel method show promising applications due to their excellent anti-reflective properties. However, in complex environments such as medical devices, the surface of porous anti-reflective coatings easily becomes a breeding ground for microorganisms. This not only reduces optical performance but also increases the risk of disease transmission. Especially in humid environments, microbial growth is even easier, and moisture significantly reduces the coating's transmittance. Therefore, functionalizing inorganic nanoparticle anti-reflective coatings to possess anti-fogging and antibacterial properties is a crucial step in expanding their applications.
[0003] A promising recent strategy involves incorporating antibacterial metal nanoparticles (NPs) (e.g., Ag-NPs, Zn-NPs, and Cu-NPs) into coatings. These broad-spectrum antibacterial metal nanoparticles release metal ions upon hydrolysis, enabling them to rapidly penetrate cells and kill bacteria while preventing the development of antibiotic resistance. This has proven effective in numerous fields, including medical devices, screens, and lenses.
[0004] The key to improving the antibacterial properties of coatings lies in enhancing the release efficiency of antibacterial agents at the interface. Current research largely focuses on increasing the number of metal nanoparticles in the coating to enhance the antibacterial effect. However, excessive metal nanoparticles increase the surface roughness of the coating, causing light scattering, which significantly reduces the transmittance of optical components. Simultaneously, metal nanoparticles absorb certain wavelengths of light; for example, Ag-NPs absorb light at 400-500 nm. Furthermore, if metal nanoparticles are directly introduced into inorganic antireflective coatings, their bonding with the coating is weak, easily agglomerating into larger particles, which also reduces the specific surface area of the antibacterial agent, thereby decreasing antibacterial efficiency and increasing diffuse reflection. Therefore, there is an urgent need to develop an effective method to prepare hydrophilic coatings that possess both high antireflective capacity and antibacterial properties. Summary of the Invention
[0005] The purpose of this invention is to provide a method for preparing a superhydrophilic antibacterial and antireflective coating, and the antibacterial and antireflective coating itself. By establishing a secondary reaction platform on the surface of an inorganic nano-coating, antibacterial ions are reduced in situ to antibacterial nanoparticles on the surface of the antireflective coating, thus preparing an antibacterial and antireflective coating. This solves the problems of antireflective coatings being easily contaminated by microorganisms and the significant decrease in light transmittance after the introduction of metallic antibacterial agents. This superhydrophilic antibacterial and antireflective functionalized coating includes an inorganic nanoparticle layer, a polydopamine layer, and an antibacterial nanoparticle layer. The high porosity and low refractive index of the inorganic nano-coating give it excellent antireflective properties. By reducing antibacterial nanoparticles in situ on its surface, the coating possesses both antibacterial and antireflective properties, solving the problem that existing antireflective coatings cannot resist microbial contamination.
[0006] To address the aforementioned technical problems, this invention provides a method for preparing a superhydrophilic antibacterial and antireflective coating, comprising the following steps:
[0007] Step 1: Add silane or titanate to an appropriate amount of solvent, stir and hydrolyze for 0.5-24 hours under the catalysis of acid or base catalyst; then age for more than 24 hours to obtain inorganic nanoparticle sol.
[0008] Step 2: The inorganic nanoparticle sol obtained in Step 1 is coated onto the substrate surface, dried at room temperature, and then calcined at high temperature to prepare an inorganic nanoparticle anti-reflective coating.
[0009] Alternatively, prepare multiple inorganic nanoparticle sols according to step one, and then uniformly mix the multiple inorganic nanoparticle sols in any proportion to obtain a mixed inorganic nanoparticle sol; coat the mixed inorganic nanoparticle sol onto the surface of the substrate, dry it at room temperature, and then calcine it at high temperature to prepare an inorganic nanoparticle anti-reflective coating.
[0010] Step 3: Place the inorganic nanoparticle antireflective coating prepared in Step 2 into an aqueous solution of dopamine-tris(hydroxymethyl)aminomethane hydrochloride. After a first predetermined time, remove it, rinse and dry it to obtain a semi-finished inorganic nanoparticle antireflective coating.
[0011] Step 4: Place the inorganic nanoparticle anti-reflective coating semi-finished product in an antibacterial metal salt solution. After a second predetermined time, remove it, rinse, and dry it to obtain a superhydrophilic antibacterial and anti-reflective coating.
[0012] In the inorganic nanoparticle sol prepared in step one, the molar ratio of each substance is: silane: titanate: solvent: catalyst = 0-10: 0-10: 10-100: 1-5.
[0013] According to the above preparation method, the present invention also provides an antibacterial and antireflective coating, which is a three-layer coating system, comprising: a bottom layer of porous nano-silica or titanium dioxide, a middle layer of dopamine, and a top layer of nano-silver particles.
[0014] Compared with the prior art, the beneficial effects of the present invention are:
[0015] (1) The anti-reflective coating prepared by the present invention has excellent anti-reflective properties, with an average light transmittance greater than 96%. The high porosity and low refractive index of the inorganic porous nano-coating give it excellent anti-reflective properties; the deposition of polydopamine reduces the surface roughness of the coating, thereby reducing light scattering and further increasing the transmittance; under the effect of in-situ reduction of polydopamine, the antibacterial nanoparticles are uniformly anchored on the coating surface, reducing the negative impact of metal nanoparticles on the transmittance.
[0016] (2) The coating has super antibacterial properties. The antibacterial efficiency of the coating against various bacteria / fungi such as Escherichia coli, Staphylococcus aureus, and Pseudomonas aeruginosa can reach 100%. The uniformly dispersed nano-silver particles have excellent bactericidal effect; the superhydrophilic properties of inorganic nanoparticles will form a local oxygen-rich and water-rich environment, which will accelerate the hydrolysis and activation of antibacterial nanoparticles and further enhance the activity of nano-silver.
[0017] (3) The anti-reflective coating prepared by the present invention has super-hydrophilic and anti-fogging properties and can be used in humid or water vapor environments.
[0018] (4) The anti-reflective coating prepared by the present invention has super mechanical durability and can maintain long-term antibacterial properties and anti-reflective effect.
[0019] (5) The preparation method of the present invention has the characteristics of simple process, obvious effect, good biocompatibility, energy saving and environmental protection and low cost, which is conducive to large-scale promotion and use. Attached Figure Description
[0020] Figure 1 This is a SEM image of the silica antireflective coating of Embodiment 1 of the present invention;
[0021] Figure 2 This is a SEM image of the polydopamine silica antireflective coating of Example 1 of the present invention;
[0022] Figure 3 This is a Nano-IR comparison image of the silica coating and the polydopamine silica coating of Example 1 of the present invention;
[0023] Figure 4 This is a comparison image of the AFM of the silica coating and the polydopamine silica coating in Example 1 of the present invention;
[0024] Figure 5 This is a SEM image of the antibacterial and antireflective coating of Embodiment 1 of the present invention;
[0025] Figure 6 This is an XPS image of the antibacterial and antireflective coating of Embodiment 1 of the present invention. Detailed Implementation
[0026] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0027] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.
[0028] The method for preparing the superhydrophilic antibacterial and antireflective coating of the present invention includes the following steps:
[0029] Step 1: Add silane or titanate to an appropriate amount of solvent, stir and hydrolyze for 0.5-24 hours under the catalysis of acid or base catalyst; then age for more than 24 hours to obtain inorganic nanoparticle sol.
[0030] Step 2: The inorganic nanoparticle sol obtained in Step 1 is coated onto the surface of the substrate, dried at room temperature, and then calcined at high temperature to prepare an inorganic nanoparticle anti-reflective coating.
[0031] Alternatively, prepare multiple inorganic nanoparticle sols according to step one, and then uniformly mix the multiple inorganic nanoparticle sols in any proportion to obtain a mixed inorganic nanoparticle sol; coat the mixed inorganic nanoparticle sol onto the surface of the substrate, dry it at room temperature, and then calcine it at high temperature to prepare an inorganic nanoparticle anti-reflective coating.
[0032] Step 3: Place the inorganic nanoparticle antireflective coating prepared in Step 2 into an aqueous solution of dopamine-tris(hydroxymethyl)aminomethane hydrochloride. After a first predetermined time, remove it, rinse and dry it to obtain a semi-finished inorganic nanoparticle antireflective coating.
[0033] Step 4: Place the inorganic nanoparticle anti-reflective coating semi-finished product in an antibacterial metal salt solution. After a second predetermined time, remove it, rinse, and dry it to obtain a superhydrophilic antibacterial and anti-reflective coating.
[0034] In the inorganic nanoparticle sol prepared in step one, the molar ratio of each substance is: silane: titanate: solvent: catalyst = 0-10: 0-10: 10-100: 1-5.
[0035] In a preferred embodiment, in step two, the coating method is any one of the following: pull coating, roller coating, spray coating, or spin coating.
[0036] In a preferred embodiment, the silane mentioned in step one is any one of tetraethyl orthosilicate, ethyltrimethoxysilane, or ethoxytrimethylsilane, or any combination of two or three of them;
[0037] The titanate ester mentioned in step one is any one of tetrabutyl titanate or tetraisopropyl titanate, or a combination of two.
[0038] The solvent mentioned in step one is any one of methanol, ethanol, propanol, n-butanol, octanol, pentanol, hexanol, heptanol, ethylene glycol, glycerol, propylene glycol, isopropanol, or water (H2O), or any combination of two of them.
[0039] The acid catalyst mentioned in step one is any one of hydrochloric acid, phosphoric acid, nitric acid, acetic acid, or carbonic acid, or any combination of two of them;
[0040] The alkaline catalyst mentioned in step one is any one of potassium hydroxide, sodium hydroxide, or ammonia (25%-44%), or any combination of two of them.
[0041] The step two involves calcining at a high temperature of 150℃-800℃ for 0-5 hours.
[0042] In step three, the mass ratio of DA, Tris-HCl, and H2O in the dopamine-tris(hydroxymethyl)aminomethane hydrochloride solution is 0.1-0.5:0.1-3:100, and the first predetermined time is 1-24 hours.
[0043] The silver nitrate solution mentioned in step four has a silver nitrate mass fraction of 0.1-10%, and the second predetermined time is 0.5-24h.
[0044] Example 1
[0045] (1) Preparation of Inorganic Nanoparticle Antireflective Coating
[0046] Inorganic nanoparticles were prepared using the sol-gel method. 5g of tetraethyl orthosilicate was added to 50g of ethanol and stirred for 15 min. Then, 0.12g of ammonia was added and stirring continued for 1 h. Finally, the mixture was allowed to stand for 7 days to obtain an inorganic nanosol-gel. A completely clean glass plate was immersed in the sol and pulled up at a uniform speed, dried, and sintered at 300℃ for 1 h to prepare a silica antireflective coating.
[0047] (2) Preparation of polydopamine functional layer
[0048] 0.1 g of dopamine and 0.12 g of tris(hydroxymethyl)aminomethane hydrochloric acid were added to 100 g of deionized water and stirred for 1 h to obtain a dopamine solution. The above silica antireflective coating was placed in the dopamine solution for 6 h, rinsed 3 times with deionized water, and then placed in a 50 °C oven for 3 h to prepare a polydopamine-containing silica antireflective coating.
[0049] (3) Preparation of superhydrophilic antibacterial and antireflective coating
[0050] The above-mentioned functional silica antireflective coating was placed in a 0.05 g / ml silver nitrate solution with pH=10 for 1 hour, then rinsed three times with deionized water and placed in a 40℃ oven for 24 hours to prepare a superhydrophilic antibacterial and antireflective coating.
[0051] The testing equipment included: a UV spectrophotometer, a biochemical incubator, and a plate counter.
[0052] like Figure 1 The image shown is a SEM image of the silicon dioxide antireflective coating of Embodiment 1 of the present invention; from Figure 1 It can be seen that the silica nanoparticles in the silica antireflective coating are uniformly distributed and have a particle size of about 17 nm.
[0053] like Figure 2 The image shown is a SEM image of the polydopamine silica antireflective coating of Example 1 of the present invention; Figure 2 It can be seen that the deposition of polydopamine does not change the surface morphology of silica nanoparticles, and... Figure 1 There was no significant change compared to the previous period.
[0054] like Figure 3 The image shown is a Nano-IR comparison diagram of the silica coating and the polydopamine silica coating of Example 1 of the present invention; Figure 3 It can be seen that the polydopamine coating is deposited at 1570 cm⁻¹ -1 A stretching vibration peak of polydopamine (C=N) was observed at the point. This peak was not detected on silica, indicating that polydopamine was successfully deposited on the silica coating surface.
[0055] like Figure 4The image shown is an AFM comparison diagram of the silica coating and the polydopamine silica coating of Example 1 of the present invention; from Figure 4 It can be seen that the deposition of polydopamine on the silica surface reduces the surface roughness of the coating from 5.69 nm to 3.55 nm. The reduction in coating roughness is beneficial to reducing light scattering and improving light transmittance.
[0056] like Figure 5 The image shown is a SEM image of the antibacterial and antireflective coating of Embodiment 1 of the present invention; from Figure 5 It can be seen that silver nanoparticles with a particle size range of 100-150nm are deposited on the surface of polydopamine and are evenly distributed.
[0057] like Figure 6 The image shown is an XPS image of the antibacterial and antireflective coating of Embodiment 1 of the present invention; from Figure 6 The XPS spectrum of the superhydrophilic antibacterial and antireflective coating revealed seven elemental characteristic peaks: Si2p, Si2s, C1s, Ag3d5 / 2, Ag3d3 / 2, N1s, and O1s.
[0058] Example 2
[0059] (1) Preparation of Inorganic Nanoparticle Antireflective Coating
[0060] Inorganic nanoparticles were prepared using the sol-gel method. 3g of tetraethyl orthosilicate was added to 50g of ethanol and stirred for 15 minutes. Then, 0.14g of ammonia was added and stirring continued for 1 hour. The mixture was then aged for 7 days to obtain an inorganic nanosol. This sol was sprayed onto a completely clean glass plate using a liquid spray gun, dried, and sintered at 350℃ for 2 hours to produce a silica antireflective coating.
[0061] (2) Preparation of polydopamine functional layer
[0062] 0.1 g of dopamine and 0.12 g of tris(hydroxymethyl)aminomethane hydrochloric acid were added to 100 g of deionized water and stirred for 1 h to obtain a dopamine solution. The above silica antireflective coating was placed in the dopamine solution for 6 h, rinsed 3 times with deionized water, and then placed in a 50 °C oven for 3 h to prepare a polydopamine-containing silica antireflective coating.
[0063] (3) Preparation of superhydrophilic antibacterial and antireflective coating
[0064] The above-mentioned functional silica antireflective coating was placed in a 0.1 g / ml silver nitrate solution with pH=10 for 3 h, then rinsed three times with deionized water and placed in a 40℃ oven for 24 h to prepare a superhydrophilic antibacterial and antireflective coating.
[0065] Example 3
[0066] (1) Preparation of Inorganic Nanoparticle Antireflective Coating
[0067] Inorganic nanoparticles were prepared using the sol-gel method. 5g of tetraethyl orthosilicate was added to 50g of ethanol and stirred for 15 min. Then, 0.14g of ammonia was added and stirring continued for 1 h. The mixture was then aged for 7 days to obtain an inorganic nanosol. A completely clean glass plate was placed on a spin coater, and the sol was dropped onto the plate. After rotary drying, the plate was sintered at 350℃ for 30 min to prepare a silica antireflective coating.
[0068] (2) Preparation of polydopamine functional layer
[0069] 0.1 g of dopamine and 0.12 g of tris(hydroxymethyl)aminomethane hydrochloric acid were added to 100 g of deionized water and stirred for 1 h to obtain a dopamine solution. The above silica antireflective coating was placed in the dopamine solution for 6 h, rinsed 3 times with deionized water, and then placed in a 50 °C oven for 3 h to prepare a polydopamine-containing silica antireflective coating.
[0070] (3) Preparation of superhydrophilic antibacterial and antireflective coating
[0071] The above-mentioned functional layer silica antireflective coating was placed in a 0.01 g / ml silver nitrate solution with pH=7 for 1 hour, then rinsed three times with deionized water and placed in a 40℃ oven for 24 hours to prepare a superhydrophilic antibacterial antireflective coating.
[0072] Example 4
[0073] (1) Preparation of Inorganic Nanoparticle Antireflective Coating
[0074] Inorganic nanoparticles were prepared using the sol-gel method. 6g of tetraethyl orthosilicate was added to 50g of isopropanol and stirred for 15 min. Then, 0.14g of ammonia was added and stirring continued for 1 h. The mixture was then aged for 7 days to obtain an inorganic nanosol. This sol was sprayed onto a completely clean glass plate using a liquid spray gun, dried, and sintered at 350℃ for 2 h to prepare a silica antireflective coating.
[0075] (2) Preparation of polydopamine functional layer
[0076] 0.1 g of dopamine and 0.12 g of tris(hydroxymethyl)aminomethane hydrochloric acid were added to 100 g of deionized water and stirred for 1 h to obtain a dopamine solution. The above silica antireflective coating was placed in the dopamine solution for 6 h, rinsed 3 times with deionized water, and then placed in a 50 °C oven for 3 h to prepare a polydopamine-containing silica antireflective coating.
[0077] (3) Preparation of superhydrophilic antibacterial and antireflective coating
[0078] The above-mentioned functional silica antireflective coating was placed in a 0.05 g / ml silver nitrate solution with pH=10 for 1 hour, then rinsed three times with deionized water and placed in a 40℃ oven for 24 hours to prepare a superhydrophilic antibacterial and antireflective coating.
[0079] Example 5
[0080] (1) Preparation of Inorganic Nanoparticle Antireflective Coating
[0081] Inorganic nanoparticles were prepared using the sol-gel method. 3g of tetraethyl orthosilicate was added to 50g of ethanol and stirred for 15 minutes. Then, 0.14g of ammonia was added, and stirring continued for 1 hour. The mixture was then aged for 7 days to obtain sol A. 1g of tetraethyl orthosilicate and 7g of ethanol were added to sol A, and stirring was continued for 15 minutes. Then, 0.1g of hydrochloric acid and 0.3g of water were added, and stirring continued for 1 hour. The mixture was then aged for 7 days to obtain the final sol-gel. A completely clean glass plate was immersed in this sol, pulled up at a uniform speed, dried, and sintered at 300℃ for 3 hours to prepare a silica antireflective coating.
[0082] (2) Preparation of polydopamine functional layer
[0083] 0.1 g of dopamine and 0.12 g of tris(hydroxymethyl)aminomethane hydrochloric acid were added to 100 g of deionized water and stirred for 1 h to obtain a dopamine solution. The above silica antireflective coating was placed in the dopamine solution for 6 h, rinsed 3 times with deionized water, and then placed in a 50 °C oven for 3 h to prepare a polydopamine-containing silica antireflective coating.
[0084] (3) Preparation of superhydrophilic antibacterial and antireflective coating
[0085] The above-mentioned functional layer silica antireflective coating was placed in a 0.1 g / ml silver nitrate solution with pH=10 for 1 hour, then rinsed three times with deionized water and placed in a 40℃ oven for 24 hours to prepare a superhydrophilic antibacterial antireflective coating.
[0086] Example 6
[0087] (1) Preparation of Inorganic Nanoparticle Antireflective Coating
[0088] Inorganic nanoparticles were prepared using the sol-gel method. 5g of tetraethyl orthosilicate was added to 35g of ethanol and stirred for 15 min. Then, 1.8g of water and 0.5g of hydrochloric acid were added, and stirring continued for 1 h. The mixture was then aged for 7 days to obtain an inorganic nanosol. A completely clean glass plate was placed on a spin coater, and the sol was dropped onto the plate. After rotary drying, the plate was sintered at 300℃ for 30 min to prepare a silica antireflective coating.
[0089] (2) Preparation of polydopamine functional layer
[0090] 0.1 g of dopamine and 0.12 g of tris(hydroxymethyl)aminomethane hydrochloric acid were added to 100 g of deionized water and stirred for 1 h to obtain a dopamine solution. The above silica antireflective coating was placed in the dopamine solution for 6 h, rinsed 3 times with deionized water, and then placed in a 50 °C oven for 3 h to prepare a polydopamine-containing silica antireflective coating.
[0091] (3) Preparation of superhydrophilic antibacterial and antireflective coating
[0092] The above-mentioned functional layer silica antireflective coating was placed in a 0.01 g / ml silver nitrate solution with pH=7 for 1 hour, then rinsed three times with deionized water and placed in a 40℃ oven for 24 hours to prepare a superhydrophilic antibacterial antireflective coating.
[0093] Example 7
[0094] (1) Preparation of Inorganic Nanoparticle Antireflective Coating
[0095] Inorganic nanoparticles were prepared using the sol-gel method. 3g of tetraethyl orthosilicate was added to 50g of ethanol and stirred for 15 min. Then, 0.14g of ammonia was added and stirring continued for 1 h. The mixture was then aged for 7 days to obtain an inorganic nanosol. The inorganic nanosol was then applied uniformly to a completely clean glass plate using a mixing brush and sintered at 300℃ for 30 min to form a silica antireflective coating.
[0096] (2) Preparation of polydopamine functional layer
[0097] 0.1 g of dopamine and 0.12 g of tris(hydroxymethyl)aminomethane hydrochloric acid were added to 100 g of deionized water and stirred for 1 h to obtain a dopamine solution. The above silica antireflective coating was placed in the dopamine solution for 6 h, rinsed 3 times with deionized water, and then placed in a 50 °C oven for 3 h to prepare a polydopamine-containing silica antireflective coating.
[0098] (3) Preparation of superhydrophilic antibacterial and antireflective coating
[0099] The above-mentioned functional layer silica antireflective coating was placed in a 0.1 g / ml silver nitrate solution with pH=10 for 1 hour, then rinsed three times with deionized water and placed in a 40℃ oven for 24 hours to prepare a superhydrophilic antibacterial antireflective coating.
[0100] Example 8
[0101] (1) Preparation of Inorganic Nanoparticle Antireflective Coating
[0102] Inorganic nanoparticles were prepared using the sol-gel method. 3g of tetrabutyl titanate was added to 50g of n-butanol and stirred for 15 min. Then, 0.14g of water and 0.15g of hydrochloric acid were added, and stirring continued for 1 h. The mixture was then aged for 7 days to obtain an inorganic nanosol. A completely clean glass plate was immersed in this sol-gel, uniformly stretched, dried, and sintered at 400℃ for 1 h to prepare a titanium dioxide antireflective coating.
[0103] (2) Preparation of polydopamine functional layer
[0104] 0.1 g of dopamine and 0.12 g of tris(hydroxymethyl)aminomethane hydrochloric acid were added to 100 g of deionized water and stirred for 1 h to obtain a dopamine solution. The above titanium dioxide antireflective coating was placed in the dopamine solution for 6 h, rinsed three times with deionized water, and then placed in a 50 °C oven for 3 h to prepare a polydopamine-containing titanium dioxide antireflective coating.
[0105] (3) Preparation of superhydrophilic antibacterial and antireflective coating
[0106] The above-mentioned functional titanium dioxide antireflective coating was placed in a 0.1 g / ml silver nitrate solution with pH=10 for 1 hour, then rinsed three times with deionized water and placed in a 40℃ oven for 24 hours to prepare a superhydrophilic antibacterial and antireflective coating.
[0107] Example 9
[0108] (1) Preparation of Inorganic Nanoparticle Antireflective Coating
[0109] Inorganic nanoparticles were prepared using the sol-gel method. 7g of tetraethyl orthosilicate was added to 50g of ethanol and stirred for 15 min. Then, 0.18g of ammonia was added and stirring continued for 1 h. The mixture was then aged for 7 days to obtain an inorganic nanosol. A completely clean glass plate was immersed in this sol-gel, uniformly stretched, dried, and sintered at 380℃ for 1 h to prepare a silica antireflective coating.
[0110] (2) Preparation of polydopamine functional layer
[0111] 0.1 g of dopamine and 0.12 g of tris(hydroxymethyl)aminomethane hydrochloric acid were added to 100 g of deionized water and stirred for 1 h to obtain a dopamine solution. The above silica antireflective coating was placed in the dopamine solution for 6 h, rinsed 3 times with deionized water, and then placed in a 50 °C oven for 3 h to prepare a polydopamine-containing silica antireflective coating.
[0112] (3) Preparation of superhydrophilic antibacterial and antireflective coating
[0113] The above-mentioned functional layer silica antireflective coating was placed in a 0.01 g / ml silver nitrate solution with pH=7 for 1 hour, then rinsed three times with deionized water and placed in a 40℃ oven for 24 hours to prepare a superhydrophilic antibacterial antireflective coating.
[0114] Example 10
[0115] (1) Preparation of Inorganic Nanoparticle Antireflective Coating
[0116] Inorganic nanoparticles were prepared using the sol-gel method. 3g of tetraethyl orthosilicate was added to 50g of ethanol and stirred for 15 minutes. Then, 0.14g of ammonia was added and stirring continued for 1 hour. The mixture was then aged for 7 days to obtain an inorganic nanosol. A completely clean glass plate was immersed in this sol-gel, uniformly stretched, dried, and sintered at 300℃ for 1 hour to prepare a silica antireflective coating.
[0117] (2) Preparation of polydopamine functional layer
[0118] 0.1 g of dopamine and 0.12 g of tris(hydroxymethyl)aminomethane hydrochloric acid were added to 100 g of deionized water and stirred for 1 h to obtain a dopamine solution. The above silica antireflective coating was placed in the dopamine solution for 6 h, rinsed 3 times with deionized water, and then placed in a 50 °C oven for 3 h to prepare a polydopamine-containing silica antireflective coating.
[0119] (3) Preparation of superhydrophilic antibacterial and antireflective coating
[0120] The above-mentioned functional layer silica antireflective coating was placed in a 0.1 g / ml silver nitrate solution with pH=10 for 1 hour, then rinsed three times with deionized water and placed in a 40℃ oven for 24 hours to prepare a superhydrophilic antibacterial antireflective coating.
[0121] Example 11
[0122] (1) Preparation of Inorganic Nanoparticle Antireflective Coating
[0123] Inorganic nanoparticles were prepared using the sol-gel method. 5g of ethyltrimethoxysilane was added to 50g of isopropanol and stirred for 15 min. Then, 0.14g of ammonia was added and stirring continued for 1 h. The mixture was then aged for 7 days to obtain an inorganic nanosol. A completely clean glass plate was immersed in this sol-gel, uniformly stretched, dried, and sintered at 320℃ for 1 h to prepare a silica antireflective coating.
[0124] (2) Preparation of polydopamine functional layer
[0125] 0.2 g of dopamine and 0.3 g of tris(hydroxymethyl)aminomethane hydrochloric acid were added to 100 g of deionized water and stirred for 1 h to obtain a dopamine solution. The above silica antireflective coating was placed in the dopamine solution for 6 h, rinsed 3 times with deionized water, and then placed in a 50 °C oven for 3 h to prepare a polydopamine-containing silica antireflective coating.
[0126] (3) Preparation of superhydrophilic antibacterial and antireflective coating
[0127] The above-mentioned functional silica antireflective coating was placed in a 0.1 g / ml silver nitrate solution with pH = 8.5 for 1 hour, then rinsed three times with deionized water and placed in a 40°C oven for 24 hours to prepare a superhydrophilic antibacterial and antireflective coating.
[0128] Example 12
[0129] (1) Preparation of Inorganic Nanoparticle Antireflective Coating
[0130] Inorganic nanoparticles were prepared using the sol-gel method. 5g of tetraisopropyl titanate was added to 57g of ethanol and stirred for 15min. Then, 2.0g of water and 0.6g of hydrochloric acid were added, and stirring continued for 1h. The mixture was then aged for 7 days to obtain an inorganic nanosol. A completely clean glass plate was immersed in this sol-gel, uniformly stretched, dried, and sintered at 380℃ for 1h to produce a titanium dioxide antireflective coating.
[0131] (2) Preparation of polydopamine functional layer
[0132] 0.1 g of dopamine and 0.2 g of tris(hydroxymethyl)aminomethane hydrochloric acid were added to 100 g of deionized water and stirred for 1 h to obtain a dopamine solution. The above titanium dioxide antireflective coating was placed in the dopamine solution for 6 h, rinsed three times with deionized water, and then placed in a 50 °C oven for 3 h to prepare a polydopamine-containing silica antireflective coating.
[0133] (3) Preparation of superhydrophilic antibacterial and antireflective coating
[0134] The above-mentioned functional titanium dioxide antireflective coating was placed in a 0.01 g / ml silver nitrate solution with pH=9 for 1 hour, then rinsed three times with deionized water, and then placed in a 40℃ oven for 24 hours to prepare a superhydrophilic antibacterial and antireflective coating.
[0135] According to standard testing, the coatings in Examples 1-7 and 9-11 (with a silica coating as the base layer) have an average light transmittance greater than 95%, and an antibacterial rate of over 99.9% against Escherichia coli, Staphylococcus aureus, and Pseudomonas aeruginosa. The coatings in Examples 8 and 12 (with a titanium dioxide coating as the base layer) have an average light transmittance greater than 92%, and an antibacterial rate of over 99.9% against Escherichia coli, Staphylococcus aureus, and Pseudomonas aeruginosa.
[0136] According to the above preparation method, the present invention also prepares an antibacterial and antireflective coating, which is a three-layer coating system, comprising: a bottom layer of porous nano-silica or titanium dioxide, a middle layer of dopamine, and a top layer of nano-silver particles. The bottom layer has a film thickness of 50-300 nm; the middle layer has a film thickness of 5-100 nm; and the nano-silver particles have a particle size of 20-200 nm.
[0137] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a superhydrophilic antibacterial and antireflective coating, characterized in that, The preparation method includes the following steps: Step 1: Add silane or titanate to an appropriate amount of solvent, stir and hydrolyze for 0.5-24 hours under the catalysis of acid catalyst or base catalyst; then age for more than 24 hours to obtain inorganic nanoparticle sol. Step 2: The inorganic nanoparticle sol obtained in Step 1 is coated onto the surface of the substrate, dried at room temperature, and then calcined at high temperature to prepare an inorganic nanoparticle anti-reflective coating. Alternatively, prepare multiple inorganic nanoparticle sols according to step one, and then uniformly mix the multiple inorganic nanoparticle sols in any proportion to obtain a mixed inorganic nanoparticle sol; coat the mixed inorganic nanoparticle sol onto the surface of the substrate, dry it at room temperature, and then calcine it at high temperature to prepare an inorganic nanoparticle anti-reflective coating. Step 3: Place the inorganic nanoparticle antireflective coating prepared in Step 2 into an aqueous solution of dopamine-tris(hydroxymethyl)aminomethane hydrochloride. After a first predetermined time, remove it, rinse and dry it to obtain a semi-finished inorganic nanoparticle antireflective coating. Step 4: Place the inorganic nanoparticle anti-reflective coating semi-finished product in an antibacterial metal salt solution. After a second predetermined time, remove it, rinse, and dry it to obtain a superhydrophilic antibacterial and anti-reflective coating. In the inorganic nanoparticle sol prepared in step one, the molar ratio of each substance is: silane: titanate: solvent: catalyst = 0-10: 0-10: 10-100: 1-5; A secondary reaction platform was established on the surface of the inorganic nano-coating to enable antibacterial ions to be reduced in situ to antibacterial nanoparticles on the surface of the inorganic nanoparticle antireflective coating, thus preparing a superhydrophilic antibacterial and antireflective coating. In step two, the coating method is any one of the following: lift coating, roller coating, spray coating, or spin coating. The silane mentioned in step one is any one of tetraethyl orthosilicate, ethyltrimethoxysilane, or ethoxytrimethylsilane, or any combination of two or three of them; The titanate ester mentioned in step one is any one of tetrabutyl titanate or tetraisopropyl titanate, or a combination of two. The step two involves calcining at a high temperature of 150 ℃-800 ℃ for 0-5 h. The antibacterial metal salt solution mentioned in step four is a silver nitrate solution.
2. The method for preparing a superhydrophilic antibacterial and antireflective coating according to claim 1, characterized in that: The solvent mentioned in step one is any one of methanol, ethanol, propanol, n-butanol, octanol, pentanol, hexanol, heptanol, ethylene glycol, glycerol, propylene glycol, isopropanol, or water, or any combination of two of them.
3. The method for preparing a superhydrophilic antibacterial and antireflective coating according to claim 1, characterized in that: The acid catalyst mentioned in step one is any one of hydrochloric acid, phosphoric acid, nitric acid, and acetic acid, or any combination of two of them; The alkaline catalyst mentioned in step one is any one of potassium hydroxide, sodium hydroxide, or ammonia water, or any combination of two of them.
4. The method for preparing a superhydrophilic antibacterial and antireflective coating according to claim 1, characterized in that: In the aqueous solution of dopamine-tris(hydroxymethyl)aminomethane hydrochloride mentioned in step three, the mass ratio of DA, Tris-HCl and H2O is 0.1-0.5:0.1-3:100, and the first predetermined time is 1-24 hours.
5. The method for preparing a superhydrophilic antibacterial and antireflective coating according to claim 1, characterized in that: The silver nitrate solution mentioned in step four has a silver nitrate mass fraction of 0.1-10%, and the second predetermined time is 0.5-24h.
6. An antibacterial and antireflective coating prepared by the method according to claim 1, characterized in that, The antibacterial and antireflective coating is a three-layer system, comprising: a bottom layer of porous nano-silica or titanium dioxide, a middle layer of polydopamine, and a top layer of nano-silver particles.
7. The antibacterial and antireflective coating according to claim 6, characterized in that, The thickness of the bottom layer is 50-300 nm; the thickness of the middle layer is 5-100 nm; and the particle size of the silver nanoparticles is 20-200 nm.
Citation Information
Patent Citations
Preparation method of visible light full-waveband multilayer antireflection coating
CN102838889A
Preparation method of nano silver / poly dopamine composite membrane
CN105013336A
Anti-reflection coating with antibacterial property and preparation method thereof
CN110143764A