Composite multilayer film for secondary electron emission and method for manufacturing the same

By designing a cyclic stacked structure of different functional layers in the thin film, the problem of lattice distortion caused by doping elements was solved, achieving high secondary electron emission performance and long-term stability, which is suitable for vacuum electronic devices.

CN118326356BActive Publication Date: 2026-11-24XI AN JIAOTONG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410429639.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-10
Publication Date
2026-11-24
Estimated Expiration
2044-04-10

AI Technical Summary

Technical Problem

In existing technologies, the combination of multiple doping elements leads to lattice distortion, introduces a large number of defects, affects secondary electron emission performance and stability, and makes it difficult to meet the requirements of vacuum electronic devices for high gain and long life.

Method used

By employing a cyclic stacking design of different functional layers, composite multilayer thin films with three structures, namely A, B, and C, are formed. Through interface correction and optimal band arrangement, lattice distortion and band barriers are reduced, and electron conduction is optimized.

Benefits of technology

It improves the secondary electron emission coefficient, reduces the impact of charge accumulation under long-term particle bombardment, and enhances the stability and conductivity of the thin film, making it suitable for devices such as electron multipliers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118326356B_ABST
    Figure CN118326356B_ABST
Patent Text Reader

Abstract

The present application belongs to the technical field of vacuum electron devices and materials, and relates to a composite multilayer film for secondary electron emission, which is formed by cyclically stacking basic stack structures formed by different functional layers to realize interface modification and optimal energy band arrangement. A preparation method of the composite multilayer film is also disclosed, which comprises the following steps: mounting a cleaned substrate on a substrate holder, depositing different functional layers to obtain a first basic stack structure; and then cyclically stacking the basic stack structures according to the deposition sequence of the basic stack structures to finally obtain the composite multilayer film for secondary electron emission. Compared with a traditional gold-doped magnesium oxide film, the composite multilayer film further improves the conductivity of the composite film, reduces the significant attenuation of the secondary electron emission coefficient caused by the accumulation of charges under long-time particle bombardment, and improves the secondary electron emission coefficient of the film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of vacuum electronic devices and materials technology, specifically relating to a composite multilayer thin film for secondary electron emission and its preparation method. Background Technology

[0002] MgO, a commonly used secondary electron emission material, not only possesses a high dielectric constant and a wide band gap, reducing the likelihood of collisions between internal secondary electrons and free electrons, thus facilitating the emission of secondary electrons from the film surface, but also exhibits excellent resistance to particle bombardment, making it widely used in devices such as electron multipliers, photomultiplier tubes, and cross-field amplifiers. However, due to its insulating properties, pure MgO films experience surface charge accumulation under prolonged particle bombardment, leading to a decrease in its secondary electron emission coefficient. This makes it difficult to meet the growing demands for high gain and long lifetime in vacuum electronic devices.

[0003] Considering the close relationship between secondary electron emission performance and the morphology and microstructure of thin films, researchers have proposed to regulate secondary electron emission performance by doping pure magnesium oxide to create different vacancies, thereby altering the band gap and surface morphology. Reported doping elements can be categorized into alkaline earth metal oxides, transition metal oxides, and rare earth oxides. Among these elements, aluminum has attracted considerable research interest due to its excellent properties. As a multifunctional molecule, aluminum is not only used as a dopant in magnesium oxide films to enhance their secondary electron emission performance, but its excellent conductivity also reduces charge accumulation on the film surface. Furthermore, it can serve as a surface passivation layer to improve stability. While these methods have improved the secondary electron emission performance of the films to some extent, their conductivity remains poor, making it difficult to maintain a high secondary electron emission coefficient under prolonged particle bombardment. Therefore, researchers have attempted to improve the conductivity of pure magnesium oxide by doping it with metal elements such as gold and silver, which has somewhat improved the attenuation of secondary electron emission in the films. However, the performance of the composite thin films reported so far still needs further improvement. Not only does the secondary electron emission coefficient need to be significantly increased, but its stability under long-term particle bombardment also needs further optimization, so that it can be better applied to related devices. In order to obtain thin films with high secondary electron emission coefficient and resistance to electron bombardment, it is necessary to combine multiple doping elements to achieve performance synergy. However, simply doping different elements together will lead to severe lattice distortion, thereby introducing a large number of defects. This will not only form traps for secondary electrons, but also create band barriers that hinder electron conduction. Summary of the Invention

[0004] The purpose of this invention is to provide a composite multilayer thin film for secondary electron emission and its preparation method, which solves the problem that combining multiple dopant elements together leads to severe lattice distortion and introduces a large number of defects.

[0005] This invention is achieved through the following technical solution: This invention discloses a composite multilayer thin film for secondary electron emission. The composite multilayer thin film is formed by cyclically stacking and arranging a basic stacked structure of different functional layers to achieve interface correction and optimal band arrangement.

[0006] Furthermore, the functional layers are divided into: a MgO functional layer with a high secondary electron emission coefficient; a MgO+Al2O3 functional layer resistant to particle bombardment; and a MgO+Au functional layer with high conductivity.

[0007] Furthermore, the basic stacking order of the three functional layers is different, specifically divided into three types, referred to as structure A, structure B, and structure C; The basic stacking structure of structure A is: (MgO+Au) / (MgO+Al2O3) / MgO; The basic stacking structure of the B structure is: (MgO+Au) / (MgO+Al2O3). The basic stacking structure of C is: (MgO+Au) / MgO / (MgO+Al2O3) / MgO.

[0008] Furthermore, the total thickness of the composite multilayer film is 30-80 nm, and the total thickness of the composite multilayer film is obtained by repeatedly cycling the basic stacking structure.

[0009] This invention also discloses a method for preparing a composite multilayer thin film for secondary electron emission, comprising the following steps: S1. Clean the substrate; S2. Mount the substrate on the substrate holder and deposit different functional layers to obtain the first basic stacked structure; S3. Then, following the deposition sequence of the basic stacked structure, the composite multilayer thin film for secondary electron emission is cyclically stacked to finally obtain the composite multilayer thin film.

[0010] Furthermore, in S2, the substrate holder is placed in the reaction chamber of magnetron sputtering. Argon and oxygen are introduced during sputtering, with an argon to oxygen flow rate ratio of (8:1) to (2:1). The gas pressure in the reaction chamber is maintained at 0.1 Pa to 0.8 Pa.

[0011] Furthermore, the functional layers are divided into: a MgO functional layer with a high secondary electron emission coefficient; a MgO+Al2O3 functional layer resistant to particle bombardment; and a MgO+Au functional layer with high conductivity. When depositing the MgO functional layer, a magnesium target or a magnesium oxide target is sputtered separately using radio frequency or DC methods; When depositing the MgO+Au functional layer, the gold target and magnesium target are sputtered together using radio frequency or DC methods. During the cyclic stacking, the sputtering power of the gold target is gradually reduced to achieve time-division control of the gold content in the thin film. When depositing the MgO+Al2O3 functional layer, the aluminum target and the magnesium target are sputtered together using either radio frequency or DC methods. During the deposition of three different functional layers, the substrate temperature was maintained at 300-500 ℃.

[0012] Furthermore, the aluminum target is a pure aluminum target or an alumina target, and the magnesium target is a pure magnesium target or a magnesium oxide target.

[0013] Furthermore, the basic stacking order of the three functional layers is different, specifically divided into three types, referred to as structure A, structure B, and structure C; First, a MgO+Au functional layer is deposited, then a MgO+Al2O3 functional layer is deposited, and finally a MgO functional layer is deposited to obtain the basic stacked structure of the A structure: (MgO+Au) / (MgO+Al2O3) / MgO; First, a MgO+Au functional layer is deposited, followed by a MgO+Al2O3 functional layer, to obtain the basic stacked structure of the B structure: (MgO+Au) / (MgO+Al2O3). First, a MgO+Au functional layer is deposited, then a MgO functional layer is deposited, then a MgO+Al2O3 functional layer is deposited, and finally a MgO functional layer is deposited to obtain the basic stacked structure of C: (MgO+Au) / MgO / (MgO+Al2O3) / MgO.

[0014] Compared with the prior art, the present invention has the following beneficial technical effects: This invention discloses a composite multilayer thin film for secondary electron emission. Different dopants are designed as multiple independent functional layers. By leveraging the different characteristics of each functional layer, the structure is improved. The cyclic arrangement and combination of different functional layers achieve composite multilayer thin films with various structures. The optimal arrangement between functional layers not only passivates surface and internal defects, but also, compared to thick bulk layers, confines lattice distortion within a limited space through nanoscale thin doped functional layers, optimizing overall crystallinity and reducing band barriers, thus facilitating electron conduction and improving overall secondary electron emission performance. Compared to traditional gold-doped magnesium oxide thin films, this invention not only further improves the conductivity of the composite film and mitigates the significant attenuation of the secondary electron emission coefficient caused by charge accumulation under prolonged particle bombardment, but also increases the secondary electron emission coefficient of the film.

[0015] Furthermore, this invention specifically provides three functional layers: a MgO functional layer with a high secondary electron emission coefficient; a MgO+Al2O3 functional layer resistant to particle bombardment; and a MgO+Au functional layer with high conductivity. According to previous literature, thin films doped with different elements have varying degrees of influence on the lattice and band gap. During the stacking process of functional layers, inter-interface recombination generates defects of varying degrees. These defects act as traps for electrons during electron transport, thus affecting secondary electron emission performance. Simultaneously, stacking that does not conform to the band alignment rules creates barriers that hinder the conduction of internal electrons. Therefore, three different structures are designed, and improvements are made to each structure to achieve optimal band alignment after functional layer stacking, thereby reducing surface and internal defects and achieving excellent secondary electron emission characteristics, including improving the secondary electron emission coefficient of the thin film and optimizing its stability under long-term electron bombardment.

[0016] Therefore, it is crucial to ensure the comprehensive properties of the three functional layers while reducing defects caused by interfacial recombination and lowering band barriers. It is known that the lattice constant and band structure of magnesium oxide will change differently after being compounded with different elements, depending on the atomic size and electronic structure of the compounding elements. Au and Al elements have significant differences in both atomic size and electronic structure. Different composite layers will produce different degrees of interfacial defects and band barriers after being stacked together. Therefore, the buffer transition between layers is very important. In order to obtain the optimal band arrangement order, A structure, B structure and C structure are formed. The basic stacking structure of A structure is: (MgO+Au) / (MgO+Al2O3) / MgO; the basic stacking structure of B structure is: (MgO+Au) / (MgO+Al2O3); the basic stacking structure of C structure is: (MgO+Au) / MgO / (MgO+Al2O3) / MgO.

[0017] The results show that the preferred C-structure composite multilayer film, due to the transition of the intermediate magnesium oxide layer with similar lattice constant and band structure, provides better contact for the merging of the functional layers of the other two composite elements, thereby reducing internal defects and achieving better crystallization, reducing the capture of secondary electrons, and its effective transition between energy levels lowers the potential energy barrier, which is beneficial to the conduction of internal electrons.

[0018] C-structure composite multilayer thin films, due to the synergistic effect between various functional layers and the optimal band arrangement, integrate the characteristics of each functional layer while reducing internal defects and band barriers caused by the composite of different layers. This optimizes the overall crystallinity of the film. Not only is the secondary electron emission coefficient superior to previously reported pure magnesium oxide, magnesium oxide doped with metal, magnesium oxide co-doped with metal and other elements secondary electron emission films, but the decay rate of the secondary electron emission coefficient under long-term electron bombardment is also significantly reduced, making it applicable to the field of electron multipliers to achieve high gain and long lifetime of devices.

[0019] Furthermore, considering that a thicker film would cause electrons from the substrate to be unable to replenish the secondary electron emission layer in time, resulting in a decrease in the secondary electron emission coefficient, while a thinner film would produce a relatively lower secondary electron emission coefficient, the thickness of the composite multilayer film in this invention is controlled between 30 nm and 80 nm.

[0020] This invention uses magnetron sputtering to deposit composite multilayer films with different structures on a substrate. Based on the best secondary electron emission performance, the secondary electron emission coefficient of the composite multilayer film is further optimized and improved by controlling the sputtering power, and the decay of the secondary electron emission coefficient of the film under long-term particle bombardment is suppressed. Attached Figure Description

[0021] Figure 1 This is a schematic diagram of the basic cyclic structure of the composite multilayer thin film with structure A described in this invention; Figure 2 This is a schematic diagram of the basic cyclic structure of the composite multilayer thin film with structure B described in this invention; Figure 3 This is a schematic diagram of the basic cyclic structure of the C-structure composite multilayer thin film described in this invention; Figure 4 This is a schematic diagram of the surface roughness of the composite multilayer thin film with structure A described in this invention; Figure 5 This is a schematic diagram of the surface roughness of the composite multilayer thin film with structure B described in this invention; Figure 6 This is a schematic diagram of the surface roughness of the C-structure composite multilayer thin film described in this invention; Figure 7 This is a comparison of curves showing the secondary electron emission coefficient δ of the composite multilayer thin film with structure A described in this invention as a function of incident electron energy Ep. Figure 8 This is a comparison of curves showing the secondary electron emission coefficient δ of the composite multilayer thin film with structure B described in this invention as a function of incident electron energy Ep. Figure 9This is a comparison of curves showing the secondary electron emission coefficient δ of the C-structure composite multilayer thin film described in this invention as a function of incident electron energy Ep. Figure 10 This is a schematic diagram showing the decay of the secondary electron emission coefficient δ of the composite multilayer thin film with structure A described in this invention over time under long-term bombardment with a fixed electron energy of 200 eV. Figure 11 This is a schematic diagram showing the decay of the secondary electron emission coefficient δ of the composite multilayer thin film with structure B described in this invention over time under long-term bombardment with a fixed electron energy of 200 eV. Figure 12 This is a schematic diagram showing the decay of the secondary electron emission coefficient δ of the C-structure composite multilayer thin film described in this invention over time under long-term bombardment with a fixed electron energy of 200 eV. Detailed Implementation

[0022] To make the objectives, technical solutions, and advantages of the present invention clearer, the following detailed description is provided in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention; that is, the described embodiments are only a part of the embodiments of the present invention, and not all of them.

[0023] The components described and illustrated in the accompanying drawings and embodiments of this invention can be arranged and designed in various different configurations. Therefore, the detailed description of the embodiments of the invention provided in the following drawings is not intended to limit the scope of the claimed invention, but merely to illustrate one selected embodiment of the invention. All other embodiments obtained by those skilled in the art based on the accompanying drawings and embodiments of this invention without inventive effort are within the scope of protection of this invention.

[0024] It should be noted that the terms “comprising,” “including,” or any other variations are intended to cover non-exclusive inclusion, such that a process, element, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to the process, element, method, article, or apparatus.

[0025] To improve the electron-induced secondary electron emission performance of existing metal-doped magnesium oxide thin films (composed of a metal-doped magnesium oxide film and a surface pure magnesium oxide film) and metal-and-other-element co-doped magnesium oxide films (composed of a metal-doped magnesium oxide film and a surface magnesium oxide film with other metals or metals and other elements co-doped into a substrate oxide film), this invention uses different functional layers and designs different structures based on the arrangement and combination of different functional layers.

[0026] Three functional layers were designed: a pure magnesium oxide layer (MgO functional layer) with a high secondary electron emission coefficient; a magnesium oxide-alumina composite layer (MgO+Al2O3 functional layer) with excellent resistance to electron bombardment; and a magnesium oxide-gold composite layer (MgO+Au functional layer) with excellent conductivity. The different functional layers were sequentially deposited in a designed structural order using a sputtering method. Because the deposition time for each functional layer is relatively short, the electrons emitted when the final composite multilayer film is bombarded originate from various different functional layers. This further ensures that the secondary electron emission performance of the final composite multilayer film combines the advantages of each functional layer.

[0027] This invention discloses a method for preparing a composite multilayer thin film for secondary electron emission, comprising the following steps: S1. Clean the substrate; S2. Mount the substrate on the substrate holder and deposit different functional layers to obtain the first basic stacked structure; S3. Then, following the deposition sequence of the basic stacked structure, the composite multilayer thin film for secondary electron emission is cyclically stacked to finally obtain the composite multilayer thin film.

[0028] In S1, the selected substrate is a stainless steel substrate, an aluminum alloy substrate, or a silver substrate.

[0029] The substrate was cleaned by sonication for 10 minutes each with acetone and ethanol, then dried with high-purity argon and baked at 120°C.

[0030] In S2, the substrate holder is placed in the reaction chamber of magnetron sputtering. Argon and oxygen are introduced during sputtering, with an argon to oxygen flow rate ratio of (8:1) to (2:1). The gas pressure in the reaction chamber is maintained at 0.1 Pa to 0.8 Pa.

[0031] In S2, the substrate temperature is maintained at 300-500 ℃ when different functional layers are deposited.

[0032] The features and performance of the present invention will be further described in detail below with reference to embodiments.

[0033] Example 1 See Figure 1 Each film layer was prepared by sputtering, specifically including the following steps: 1) Clean the substrate and use radio frequency sputtering magnesium target and DC sputtering gold target to deposit a magnesium oxide composite gold functional layer (MgO+Au) on the substrate. During the deposition process, the substrate temperature is maintained at 500 ℃ and argon and oxygen are introduced at the same time. The ratio of argon to oxygen is 5:1 and the total pressure in the coating chamber is 0.2 Pa. The final thickness of the functional layer is about 0.5 nm.

[0034] 2) A magnesium oxide composite aluminum oxide functional layer (MgO+Al2O3) was deposited on the MgO+Au functional layer using radio frequency sputtering with magnesium and aluminum targets. During the deposition process, the substrate temperature was maintained at 500 ℃, and argon and oxygen were introduced simultaneously at a ratio of 5:1. The total pressure in the coating chamber was 0.2 Pa. The final thickness of the functional layer was approximately 0.5 nm.

[0035] 3) A magnesium oxide functional layer (MgO) was deposited on a MgO+Al2O3 functional layer using radio frequency sputtering with a magnesium target. During deposition, the substrate temperature was maintained at 500 °C, and argon and oxygen were simultaneously introduced at a ratio of 5:1. The total pressure in the deposition chamber was 0.2 Pa. The final thickness of the deposited functional layer was approximately 0.5 nm. The desired result was as follows: Figure 1 The basic stacking structure is shown.

[0036] 4) Following the above deposition sequence, the layers are stacked in a cycle to eventually form a composite multilayer film with structure A.

[0037] refer to Figure 4 The thin film of this structure has a relatively rough surface.

[0038] refer to Figure 7 A schematic diagram showing the variation of the secondary electron emission coefficient δ of the composite multilayer thin film with different incident electron energies. Figure 10 The graph showing the decay of the secondary emission coefficient δ of the composite multilayer film under long-term electron bombardment at a fixed 200 eV over time indicates that the structure has good resistance to electron bombardment, with the decay decreasing by only 8.4% after 2 hours.

[0039] Example 2 See Figure 2 Each film layer was prepared by sputtering, specifically including the following steps. 1) Clean the substrate and use radio frequency sputtering magnesium target and DC sputtering gold target to deposit a magnesium oxide composite gold functional layer (MgO+Au) on the substrate. During the deposition process, the substrate temperature is maintained at 500 ℃ and argon and oxygen are introduced at the same time. The ratio of argon to oxygen is 5:1 and the total pressure in the coating chamber is 0.2 Pa. The final thickness of the functional layer is about 0.5 nm.

[0040] 2) A magnesium oxide composite aluminum oxide functional layer (MgO + Al2O3) was deposited on a MgO + Au functional layer using radio frequency sputtering with magnesium and aluminum targets. During deposition, the substrate temperature was maintained at 500 °C, and argon and oxygen were simultaneously introduced at a ratio of 5:1. The total pressure in the deposition chamber was 0.2 Pa. The final thickness of the deposited functional layer was approximately 0.5 nm. The desired result was as follows: Figure 2 The basic stacking structure is shown.

[0041] 3) Following the above deposition sequence, the layers are stacked in a cycle to eventually form a composite multilayer film with structure B.

[0042] refer to Figure 5 The thin film of this structure has a relatively rough surface.

[0043] refer to Figure 8 A schematic diagram showing the variation of the secondary electron emission coefficient δ of the composite multilayer thin film with different incident electron energies. Figure 11 The graph showing the decay of the secondary emission coefficient δ of the composite multilayer film under long-term electron bombardment at a fixed 200 eV over time indicates that the structure has good resistance to electron bombardment, with the decay decreasing by only 7.3% after 2 hours.

[0044] Example 3 See Figure 3 Each film layer was prepared by sputtering, specifically including the following steps. 1) Clean the substrate and use radio frequency sputtering magnesium target and DC sputtering gold target to deposit a magnesium oxide composite gold functional layer (MgO+Au) on the substrate. During the deposition process, the substrate temperature is maintained at 500 ℃ and argon and oxygen are introduced at the same time. The ratio of argon to oxygen is 5:1 and the total pressure in the coating chamber is 0.2 Pa. The final thickness of the functional layer is about 0.5 nm.

[0045] 2) A magnesium oxide functional layer (MgO) was deposited on the MgO+Au functional layer using radio frequency sputtering on a magnesium target. During the deposition process, the substrate temperature was maintained at 500 °C, and argon and oxygen were introduced simultaneously at a ratio of 5:1. The total pressure in the coating chamber was 0.2 Pa. The final thickness of the functional layer was approximately 0.5 nm.

[0046] 3) A magnesium oxide composite aluminum oxide functional layer (MgO + Al2O3) was deposited on the MgO functional layer using radio frequency sputtering with magnesium and aluminum targets. During the deposition process, the substrate temperature was maintained at 500 ℃, and argon and oxygen were introduced simultaneously at a ratio of 5:1. The total pressure in the coating chamber was 0.2 Pa. The final thickness of the functional layer was approximately 0.5 nm.

[0047] 4) A magnesium oxide functional layer (MgO) was deposited on a MgO+Al2O3 functional layer using radio frequency sputtering with a magnesium target. During deposition, the substrate temperature was maintained at 500 °C, and argon and oxygen were simultaneously introduced at a ratio of 5:1. The total pressure in the deposition chamber was 0.2 Pa. The final thickness of the deposited functional layer was approximately 0.5 nm. The desired result was as follows: Figure 3 The basic stacking structure is shown.

[0048] 5) Following the above deposition sequence, the layers are stacked in a cycle to eventually form a C-structured composite multilayer film.

[0049] By adjusting the sputtering power of aluminum in the functional layer MgO+Al2O3 from 30 to 100 W, the maximum secondary electron emission coefficient increased from 9.02 to 10.23; under continuous electron bombardment at a voltage of 200 eV, the decay rate decreased from 19.2% to 10.04%.

[0050] refer to Figure 6 The thin film of this structure has a smooth surface with low roughness.

[0051] refer to Figure 9 A schematic diagram showing the variation of the secondary electron emission coefficient δ of the composite multilayer thin film with different incident electron energies. Figure 12 The graph showing the decay of the secondary emission coefficient δ of the composite multilayer film under long-term electron bombardment at a fixed 200 eV over time indicates that the structure not only has a high secondary electron emission coefficient, but also has good resistance to electron bombardment while ensuring a high coefficient, with a decay of 10.7% after 2 hours.

[0052] Through comparison of three embodiments, the secondary electron emission coefficients of the three structures at 200 eV are 3.88, 3.24, and 4.81, respectively. The maximum secondary electron emission coefficients are 6.90, 5.51, and 9.91, respectively. The decay rates after 2 hours of continuous electron bombardment at 200 eV are 8.4%, 7.3%, and 10.7%, respectively. Since C exhibits a high secondary electron emission coefficient while maintaining a relatively low decay rate, it is clear that the C-structured composite multilayer film is the optimal choice.

[0053] The composite multilayer thin film prepared in this invention consists of three functional layers with different properties: a magnesium oxide layer with a high secondary electron emission coefficient, a magnesium oxide composite gold layer with excellent conductivity, and a magnesium oxide composite alumina layer with excellent resistance to particle bombardment. By designing different structures, the composite multilayer thin film was synthesized, combining the comprehensive properties of different functional layers. Furthermore, the interface modification achieved through the stacking order of the different functional layers passivates internal and surface defects in the film, improves secondary electron emission performance, and the optimized bandgap lowers the barriers between bands, which is beneficial for electron conduction.

[0054] Compared to traditional gold-doped magnesium oxide thin films, this method not only further improves the conductivity of the composite film and reduces the significant attenuation of the secondary electron emission coefficient caused by charge accumulation under long-term particle bombardment, but also increases the secondary electron emission coefficient of the film.

[0055] Considering that a thicker film would cause electrons from the substrate to not be replenished to the secondary electron emission layer in time, resulting in a decrease in the secondary electron emission coefficient, while a thinner film would produce a relatively lower secondary electron emission coefficient, the thickness of the composite multilayer film in this invention is controlled between 30 nm and 80 nm.

[0056] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the specific implementation of the present invention. Any modifications or equivalent substitutions that do not depart from the spirit and scope of the present invention should be covered within the protection scope of the present invention.

Claims

1. A composite multilayer thin film for secondary electron emission, characterized in that, The composite multilayer film is formed by arranging and combining basic stacked structures of different functional layers through multiple cycles of superposition, thereby achieving interface correction and optimal band arrangement. The functional layers are divided into: a MgO functional layer with a high secondary electron emission coefficient; a MgO+Al2O3 functional layer resistant to particle bombardment; and a MgO+Au functional layer with high conductivity. In the basic stacked structure, the basic stacking order of the three functional layers is: (MgO+Au) / MgO / (MgO+Al2O3) / MgO.

2. The composite multilayer thin film for secondary electron emission according to claim 1, characterized in that, The total thickness of the composite multilayer film is 30-80 nm, and the total thickness of the composite multilayer film is obtained by repeatedly cycling the basic stacking structure.

3. The method for preparing a composite multilayer thin film for secondary electron emission as described in claim 1 or 2, characterized in that, Includes the following steps: S1. Clean the substrate; S2. Mount the substrate on the substrate holder and deposit different functional layers to obtain the first basic stacked structure; S3. Then, following the deposition sequence of the basic stacked structure, the composite multilayer thin film for secondary electron emission is cyclically stacked to finally obtain the composite multilayer thin film.

4. The preparation method according to claim 3, characterized in that, In S2, the substrate holder is placed in the reaction chamber of magnetron sputtering. Argon and oxygen are introduced during sputtering, with an argon to oxygen flow rate ratio of (8:1) to (2:1). The gas pressure in the reaction chamber is maintained at 0.1 Pa to 0.8 Pa.

5. The preparation method according to claim 3, characterized in that, When depositing the MgO functional layer, a magnesium target or a magnesium oxide target is sputtered separately using radio frequency or DC methods; When depositing the MgO+Au functional layer, the gold target and magnesium target are sputtered together using radio frequency or DC methods. During the cyclic stacking, the sputtering power of the gold target is gradually reduced to achieve time-division control of the gold content in the thin film. When depositing the MgO+Al2O3 functional layer, the aluminum target and the magnesium target are sputtered together using either radio frequency or DC methods. During the deposition of three different functional layers, the substrate temperature was maintained at 300-500 ℃.

Citation Information

Patent Citations

  • Preparation method of secondary-electron emission thin film

    CN103789730A

  • Magnesium oxide secondary electron emission thin film doped with metal and aluminum oxide and preparation method thereof

    CN107740044A