Spinneret housing for polymer fiber production and method of use thereof

By designing the spinneret housing, the shroud reduces the concentration and temperature unevenness in the coagulation zone, solves the problem of uneven coagulant concentration around the spinneret, and improves the uniformity of the filament and the quality of the polymer fiber.

CN118339331BActive Publication Date: 2026-11-24CYTEC IND INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202280079839.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-10-06
Filing Date
2022-10-04
Publication Date
2026-11-24
Estimated Expiration
2042-10-04

AI Technical Summary

Technical Problem

In existing technologies, uneven coagulant concentration around the spinneret leads to variability in filament formation, affecting the quality of polymer fibers.

Method used

The spinneret housing design includes a flanged cylindrical wall, a coaxial cylindrical tube, and a shroud. The shroud extends beyond the far end of the flange to reduce the concentration gradient and temperature inhomogeneity in the solidification zone.

Benefits of technology

It significantly reduces the variability of filament diameter and roundness, and improves the uniformity and quality of polymer fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004869589990000161
    Figure BDA0004869589990000161
  • Figure HDA0004869590000000011
    Figure HDA0004869590000000011
  • Figure HDA0004869590000000021
    Figure HDA0004869590000000021
Patent Text Reader

Abstract

This disclosure relates to a spinneret housing for producing polymer fibers, such as large-tow polymer fibers, which are typically used in the manufacture of carbon fibers. This disclosure also relates to a system including the spinneret housing, and a method for producing polymer fibers using such a system. The produced polymer fibers can be used to manufacture carbon fibers, which can be used as structural components in composite materials relevant to many fields, such as aerospace, marine, and automotive industries.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-references to related applications

[0002] This application claims priority to U.S. Provisional Patent Application No. 63 / 252,673, filed October 6, 2021, which is incorporated herein by reference. Technical Field

[0003] This disclosure relates to a spinneret housing for producing polymer fibers, such as large-tow polymer fibers, which are typically used in the manufacture of carbon fibers. This disclosure also relates to a system including the spinneret housing, and a method for producing polymer fibers using such a system. The produced polymer fibers can be used to manufacture carbon fibers, which can be used as structural components in composite materials relevant to many fields, such as aerospace, marine, and automotive industries. Background Technology

[0004] Carbon fiber has been used in a variety of applications due to its desirable properties such as high strength and stiffness, high chemical resistance, and low thermal expansion. For example, carbon fiber can be formed into structural parts that combine high strength and high stiffness while being significantly lighter than metal parts with equivalent properties. Carbon fiber is increasingly being used as structural components in composite materials for aerospace, marine, and automotive applications. In particular, composite materials in which carbon fiber acts as a reinforcing material in a resin or ceramic matrix have been developed.

[0005] Carbon fibers derived from acrylonitrile are generally produced through a series of manufacturing steps or stages, including polymerization, spinning, drawing and / or washing, oxidation, and carbonization. Polyacrylonitrile (PAN) polymer is currently the most widely used precursor for carbon fibers. During the polymerization stage, acrylonitrile (AN), optionally containing one or more comonomers, is converted into a PAN polymer. The PAN polymer is then subjected to spinning, drawing and / or washing, oxidation, and carbonization to produce carbon fibers.

[0006] Since over 90% of carbon fibers are derived from PAN polymers, it is important to identify controllable parameters in the polymer properties that affect downstream processes, with the aim of achieving faster, lower-cost, and / or easier manufacturing of carbon fibers, especially large-tow carbon fibers.

[0007] In the spinning and coagulation steps, the polymer spinning solution is extruded through a spinneret into a coagulation bath, where the polymer coagulates to form fiber bundles or filaments. The volume of the fiber bundle decreases continuously along the coagulation bath, and the used coagulant is extruded from it. This solvent-rich liquid tends to recycle into the fiber coagulant region, which is essentially the first few inches from the spinneret face. Due to the geometry of the coagulation bath and the immersed spinneret assembly, the laminar coagulant flow around the spinneret is non-uniform, and the return rate of the used coagulant also varies, resulting in non-uniform solvent concentration around the spinneret. This concentration gradient around the coagulation region causes variability in filament formation.

[0008] Therefore, there is a continued need for apparatus and methods for producing polymer fibers, particularly large tow fibers, that can reduce or eliminate the concentration gradient that occurs around the solidification zone during the solidification step, thereby reducing or eliminating the variability in filament formation. Summary of the Invention

[0009] This objective, and other objectives that will become apparent from the following detailed description, are achieved, in whole or in part, by the apparatus, method and / or process disclosed herein.

[0010] In a first aspect, this disclosure relates to a spinneret housing having a body adapted to typically detachably secure a spinneret or spinneret assembly, the body comprising:

[0011] A flanged cylindrical wall extending from the main body, wherein the flange protrudes radially inward at the distal portion of the wall;

[0012] A cylindrical tube surrounding the body, wherein the tube is coaxial with the flanged cylindrical wall and has a diameter larger than that of the flanged cylindrical wall; and

[0013] A fairing extends from the cylindrical tube surrounding the body, wherein the fairing extends beyond the distal end of the flanged cylindrical wall.

[0014] In a second aspect, this disclosure relates to a system for producing polymer fibers, the system comprising:

[0015] a) The spinneret housing described herein;

[0016] b) Polymer spinning solution supply line;

[0017] c) Spinnerets or spinneret assemblies, typically used for large filament bundles; and

[0018] d) A coagulation bath containing coagulation liquid.

[0019] In a third aspect, this disclosure relates to a method for producing polymer fibers, the method comprising:

[0020] a') Provide the system described herein; and

[0021] b') The polymer spinning solution is spun into the coagulation bath, and the polymer spinning solution is supplied to the spinneret or spinneret assembly through the polymer spinning solution supply line.

[0022] In the fourth aspect, this disclosure relates to one or more polymer fibers produced as described herein.

[0023] In a fifth aspect, this disclosure relates to a method for producing carbon fiber, the method comprising:

[0024] (i) Providing the polymer fibers described herein or producing polymer fibers according to the methods described herein;

[0025] (ii) The polymer fiber produced in step (i) is oxidized to form a stable carbon fiber precursor fiber and then the stable carbon fiber precursor fiber is carbonized to produce the carbon fiber.

[0026] In a sixth aspect, this disclosure relates to a composite material comprising carbon fibers produced according to the methods described herein and a matrix resin. Attached Figure Description

[0027] Figure 1 A front perspective view of an embodiment of the spinneret housing described herein is shown.

[0028] Figure 2 A rear perspective view of an embodiment of the spinneret housing described herein is shown.

[0029] Figure 3 An exploded view of an embodiment of the spinneret housing described herein is shown.

[0030] Figure 4 The filament diameters, including standard deviations, are shown for white fiber bundles manufactured using and without the spinneret housing described herein.

[0031] Figure 5 The roundness, including standard deviation, of white fiber bundles manufactured using and without the spinneret housing described herein is shown. Detailed Implementation

[0032] As used herein, unless otherwise stated, the terms “a / an” or “the” mean “a / an or more / multiple” or “at least one / a” and are used interchangeably.

[0033] As used in this article, the term “and / or” in phrases in the form of “A and / or B” means A alone, B alone, or A and B together.

[0034] As used herein, the term "comprises" includes "consistsessentially of" and "consists of". The term "comprising" includes "consisting essentially of" and "consisting of". "Comprising", synonymous with "including", "containing", or "characterized by", is intended to be inclusive or open-ended and does not exclude additional, unlisted elements or steps. The transitional phrase "consisting essentially of" includes specific materials or steps that do not materially affect the essential characteristics or function of the described composition, process, method, or article. The transitional phrase "consisting of" excludes any unspecified elements, steps, or components.

[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this specification pertains.

[0036] As used herein, and unless otherwise specified, the terms “about” or “approximately” mean an acceptable error for a particular value as determined by one of ordinary skill in the art, which depends in part on how the value is measured or determined. In some embodiments, the terms “about” or “approximately” mean within 1, 2, 3, or 4 standard deviations. In some embodiments, the terms “about” or “approximately” mean within 50%, 20%, 15%, 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, 0.5%, or 0.05% of a given value or range.

[0037] Furthermore, it should be understood that any numerical ranges listed herein are intended to include all subranges included therein. For example, the range "1 to 10" is intended to include and encompass all subranges between the listed minimum value of 1 and the listed maximum value of 10; that is, a minimum value equal to or greater than 1 and a maximum value equal to or less than 10. Because the disclosed numerical ranges are continuous, they include every value between the minimum and maximum values. Unless otherwise clearly indicated, the various numerical ranges specified in this application are approximate values.

[0038] The terms and phrases “invention,” “present invention,” “instant invention,” and similar terms and phrases used herein are non-limiting and are not intended to limit the subject matter of the invention to any single embodiment, but rather to include all possible embodiments as described.

[0039] In a first aspect, this disclosure relates to a spinneret housing having a body adapted to typically detachably secure a spinneret or spinneret assembly, the body comprising:

[0040] A flanged cylindrical wall extending from the main body, wherein the flange protrudes radially inward at the distal portion of the wall;

[0041] A cylindrical tube surrounding the body, wherein the tube is coaxial with the flanged cylindrical wall and has a diameter larger than that of the flanged cylindrical wall; and

[0042] A fairing extends from the cylindrical tube surrounding the body, wherein the fairing extends beyond the distal end of the flanged cylindrical wall.

[0043] An exemplary embodiment of the spinneret housing is in Figure 1 and Figure 2 A spinneret housing 100 is shown in the image. The spinneret housing 100 includes a body 101 comprising a hollow interior shaped to receive and / or secure a spinneret or spinneret assembly, and a rear cover 102. The spinneret or spinneret assembly can be permanently or removably, typically removably, secured within the spinneret housing. The body 101 also includes a flanged cylindrical wall 104 extending from the body, wherein a flange 103 projects radially inward at a distal portion of the wall; a cylindrical tube 105 surrounds the body. A shroud 106 extends from the cylindrical tube surrounding the body beyond the distal end of the flanged cylindrical wall.

[0044] like Figure 2 As shown, the cylindrical tube 105 is coaxial with the flanged cylindrical wall and has a diameter larger than that of the flanged cylindrical wall. The cylindrical tube 105 and the body 101 provide one or more openings 107 that allow the coagulated liquid to flow through and around the spinneret or spinneret assembly.

[0045] During spinning and coagulation, the volume of the fiber bundle extruded through the spinneret decreases continuously along the coagulation bath, and the used coagulant is extruded. This solvent-rich liquid tends to recirculate to the fiber coagulant region, which is essentially a few inches from the spinneret face. Due to the geometry of the coagulation bath and the immersed spinneret assembly, the laminar coagulant flow around the spinneret is non-uniform, and the return rate of the used coagulant also varies, resulting in non-uniform solvent concentration around the spinneret. This concentration gradient around the coagulation region causes variability in filament formation. The presence of the shroud 106 serves to eliminate the formation of the concentration gradient around the coagulation region, thereby reducing or eliminating the variability in filament formation. When the spinning solution and coagulation bath temperatures differ, the shroud of the spinneret housing also reduces temperature non-uniformity in the coagulation bath around the spinneret due to its thermal insulation effect.

[0046] The shape of the fairing is not particularly limited, as long as it extends beyond the distal end of the flanged cylindrical wall, which is typically an approximation of the spinneret face. In embodiments, the fairing has a cylindrical shape, a truncated conical shape, or a combination thereof. In one embodiment, the fairing has a truncated conical shape.

[0047] As will be understood by those skilled in the art, "truncated cone" refers to the shape of a truncated cone. In other words, "truncated cone" refers to a shape formed by cutting a portion of a cone between one or two planes (typically parallel planes). This truncated cone shape can be symmetrical or asymmetrical. When the truncated cone shape is symmetrical, the cone derived from this shape is a right cone, i.e., its apex lies on an axis perpendicular to the center of the cone's base, and the cone is typically circular. In this case, the angles formed by the lateral faces and the base of the truncated cone shape are the same throughout the shape. When the truncated cone shape is asymmetrical, the cone derived from this shape is an oblique cone, i.e., its apex is not on an axis perpendicular to the center of the cone's base. In this case, the angles formed by the lateral faces and the base of the truncated cone shape are not the same throughout the shape.

[0048] The fairing can be a combination of cylindrical and truncated conical shapes. In such a configuration, for example, the fairing may initially extend from the body in a cylindrical shape and then change to a truncated conical shape.

[0049] The size of the fairing is not particularly limited. However, in some embodiments, the length of the fairing, measured from the face of the flanged cylindrical wall to the distal opening, is 10 to 100 mm, typically 15 to 40 mm. In some embodiments, the diameter of the distal opening of the fairing is 100 to 200 mm, typically 150 to 190 mm, and more typically 160 to 190 mm.

[0050] A spinneret housing can be a combination of two or more parts fixed together. This combination of two or more parts can be permanently fixed together. However, it is advantageous to fix two or more parts together so that the parts can be separated at a desired time (e.g., for maintenance, repair, replacement of one or more parts, or for removal or replacement of the spinneret). Figure 3 As shown, the exemplary spinneret housing 200 may be an assembly of a body 201 including a hollow interior shaped to receive and / or secure a spinneret or spinneret assembly 300 and a rear cover 202. The body 201 also includes a flanged cylindrical wall 203 extending from the body, wherein a flange 204 projects radially inward at a distal portion of the wall; a cylindrical tube 205 surrounds the body. A shroud 206 extends from the cylindrical tube surrounding the body beyond the distal end of the flanged cylindrical wall.

[0051] The fairing can be a permanent extension of a cylindrical tube, such as Figure 3 As shown, it may be detachable, such as Figure 2 As shown. In this embodiment, the fairing is removable. The fairing can be removably attached to the cylindrical tube using any means known to those skilled in the art, such as screws, clips, magnets, etc.

[0052] The spinneret housing can be made of materials known to those skilled in the art. Exemplary materials include, but are not limited to, metals such as iron, cast iron, copper, brass, aluminum, titanium, carbon steel, stainless steel, and alloys thereof; and polymers such as thermosetting and thermoplastic resins. Exemplary thermosetting resins include, but are not limited to, epoxy resins, oxetine, vinyl ester resins, cyanate ester resins, isocyanate-modified epoxy resins, phenolic resins, furan resins, benzoxazine, formaldehyde condensation resins (such as those with urea, melamine, or phenol), polyesters, acrylic resins, mixtures, blends, and combinations thereof. Exemplary thermoplastic polymers include, but are not limited to, acrylonitrile butadiene styrene (ABS), polypropylene, polystyrene, polyvinyl chloride, polylactic acid, polyamides (PA) such as aliphatic polyamides and semi-aromatic polyamides; polyimide (PI), polyaryletherketone (PAEK), polyamide-imide (PAI), polyarylene sulfide (PAS) such as polyphenylene sulfide (PPS); polyarylether sulfone (PAES), polyetheretherketone (PEEK), fluoropolymers (FP) such as polyvinylidene fluoride; polycarbonate, and combinations thereof.

[0053] In a second aspect, this disclosure relates to a system for producing polymer fibers, the system comprising:

[0054] a) The spinneret housing described herein;

[0055] b) Polymer spinning solution supply line;

[0056] c) Spinnerets or spinneret assemblies, typically used for large filament bundles; and

[0057] d) A coagulation bath containing coagulation liquid.

[0058] The system described herein is used to produce polymer fibers, typically for spinning a polymer spinning solution, or "spinning dope," into a coagulation bath. A spinneret or spinneret assembly is connected to a polymer spinning solution supply line, which is used to deliver the polymer spinning solution from a polymer spinning solution source (such as a storage tank containing the polymer spinning solution) to the spinneret by the action of one or more pumps. The polymer fibers are then coagulated in a coagulation bath containing a coagulation solution.

[0059] In embodiments, the spinneret or spinneret assembly is typically detachably secured within the spinneret housing.

[0060] In this embodiment, the polymer spinning solution supply line is connected to the inlet of the spinneret.

[0061] In a third aspect, this disclosure relates to a method for producing polymer fibers, the method comprising:

[0062] a') Provide the system described herein; and

[0063] b') The polymer spinning solution is spun into the coagulation bath, and the polymer spinning solution is supplied to the spinneret or spinneret assembly through the polymer spinning solution supply line.

[0064] During the manufacture of polymer fibers, such as those used in downstream processes for manufacturing carbon fibers, the polymer solution (i.e., the spinning "dosage") is typically spun into a coagulation bath. The spinning dosage may have a polymer concentration of at least 10 wt% by weight, typically from about 16 wt% to about 28 wt%, and more typically from about 19 wt% to about 24 wt% based on the total weight of the solution. The dosage is filtered and extruded through orifices in a spinneret (typically made of metal) into a liquid coagulation bath for polymer to form filaments. The spinneret orifices determine the desired fiber filament count (e.g., 3,000 orifices for 3K carbon fibers). In examples, the spinneret is used for large tow fibers, typically 24K to 50K fibers.

[0065] The coagulation bath used in this method is a mixture of solvent and non-solvent. Water or alcohol is typically used as the non-solvent. Suitable solvents include those described herein. In examples, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, or mixtures thereof are used as solvents. In another example, dimethyl sulfoxide is used as the solvent. The ratio of solvent to non-solvent and the bath temperature are not particularly limited and can be adjusted according to known methods to achieve a desired curing rate of the newly extruded filaments during coagulation. However, the coagulation bath typically contains 40 wt% to 85 wt% of one or more solvents, with the balance being a non-solvent, such as water or alcohol. In one embodiment, the coagulation bath contains 40 wt% to 70 wt% of one or more solvents, with the balance being a non-solvent. In another embodiment, the coagulation bath contains 50 wt% to 85 wt% of one or more solvents, with the balance being a non-solvent.

[0066] Typically, the temperature of the coagulation bath ranges from 0°C to 80°C. In one embodiment, the temperature of the coagulation bath ranges from 30°C to 80°C. In another embodiment, the temperature of the coagulation bath ranges from 0°C to 20°C.

[0067] To examine the fiber bundles, cross-sectional images of the bundles are obtained using a digital microscope, and then image analysis software is used to determine the filament diameter and its corresponding distribution. The distribution data is then analyzed using statistical analysis software (such as JMP) to determine filament variability. The cross-sectional shape of the filaments is analyzed using image analysis software to determine filament roundness. Filament roundness is typically normalized so that values ​​range from 0 to 1. A filament roundness of 1 is considered the ideal case for a circle.

[0068] In the embodiments, the variability of filament diameter and / or roundness is reduced by 5% to 50%, typically 10% to 40%, and more typically 20% to 25% compared to the variability of filament diameter and / or roundness obtained in a method without the spinneret housing.

[0069] In the fourth aspect, this disclosure relates to one or more polymer fibers produced as described herein.

[0070] In the embodiments, the filament diameter is 1 to 50 μm, typically 7 to 25 μm, more typically 9 to 20 μm, and even more typically 10 to 16 μm.

[0071] In the embodiments, the variability of the filament diameter is less than 2.1, typically less than 2.

[0072] In the embodiments, the filament roundness is 0.75 to 1, typically 0.75 to 0.85.

[0073] In the embodiments, the variability of filament roundness is less than 0.07.

[0074] In a fifth aspect, this disclosure relates to a method for producing carbon fiber, the method comprising:

[0075] (i) Providing the polymer fibers described herein or producing polymer fibers according to the methods described herein;

[0076] (ii) The polymer fiber produced in step (i) is oxidized to form a stable carbon fiber precursor fiber and then the stable carbon fiber precursor fiber is carbonized to produce the carbon fiber.

[0077] The polymer fibers described herein or produced according to the methods described herein can be oxidized to form stable carbon fiber precursor fibers, and the stable carbon fiber precursor fibers can then be carbonized to produce carbon fibers.

[0078] During the oxidation stage, polymer fibers are fed under tension through one or more dedicated ovens, each at a temperature of 150°C to 300°C, typically 200°C to 280°C, and more typically 220°C to 270°C. Heated air is fed into each oven. The polymer fibers are conveyed through the one or more ovens at a rate of 4 to 100 fpm, typically 30 to 75 fpm, and more typically 50 to 70 fpm.

[0079] The oxidation process combines oxygen molecules from the air with the fiber and initiates cross-linking of the polymer chains, thereby increasing the fiber density to 1.3 g / cm³. 3 Up to 1.4 g / cm 3 During the oxidation process, the tension applied to the fiber generally controls the fiber to be stretched or contracted at a draw ratio of 0.8 to 1.35, typically 1.0 to 1.2. When the draw ratio is 1, there is no stretching. And when the draw ratio is greater than 1, the applied tension stretches the fiber. This oxidized fiber, typically PAN fiber, has an infusible ladder-shaped aromatic molecular structure and is ready for carbonization.

[0080] Carbonization leads to the crystallization of carbon molecules and thus produces finished carbon fibers with a carbon content greater than 90%. The carbonization of oxidized or stabilized carbon fiber precursor fibers occurs in an inert (oxygen-free) atmosphere, typically a nitrogen atmosphere, within one or more specially designed furnaces. The oxidized carbon fiber precursor fibers are then passed through one or more ovens, each heated to a temperature ranging from 300°C to 1650°C, typically from 1100°C to 1450°C.

[0081] The adhesion between the matrix resin and carbon fibers is a crucial standard in carbon fiber reinforced polymer composites. Therefore, during the manufacturing process of carbon fibers, surface treatments can be performed after oxidation and carbonization to enhance this adhesion.

[0082] Surface treatment may involve traction carbonized fibers through an electrolytic bath containing an electrolyte such as ammonium bicarbonate or sodium hypochlorite. The chemicals in the electrolytic bath etch or roughen the fiber surface, thereby increasing the surface area available for interfacial fiber / matrix bonding and adding reactive chemical groups.

[0083] Next, the carbon fibers can be subjected to sizing, in which a sizing coating (e.g., an epoxy-based coating) is applied to the fibers. Sizing can be performed by passing the fibers through a sizing bath containing a liquid coating material. Sizing protects the carbon fibers during processing and finishing into intermediate forms such as dry fabrics and prepregs. Sizing also holds the filaments together in individual bundles to reduce fuzz, improve processability, and increase the interfacial shear strength between the fibers and the matrix resin.

[0084] After applying the adhesive, the coated carbon fiber is dried and then wound onto a winding tube.

[0085] Those skilled in the art will understand that processing conditions (including the composition of the spinning solution and coagulation bath, the total bath volume, stretching, temperature, and filament speed) can be modified to provide filaments with desired structure and denier without departing from the spirit of this disclosure.

[0086] In a sixth aspect, this disclosure relates to a composite material comprising carbon fibers produced according to the methods described herein and a matrix resin.

[0087] Composite materials can be manufactured by molding preforms containing carbon fibers produced according to the methods described herein and by infusing the preforms with thermosetting resins in a variety of liquid molding methods. Liquid molding methods that can be used include, but are not limited to, vacuum-assisted resin transfer molding (VARTM), in which resin is infused into the preform using a pressure differential created by a vacuum. Another method is resin transfer molding (RTM), in which resin is infused into the preform under pressure in a closed mold. A third method is resin film infusion (RFI), in which a semi-solid resin is placed under or on top of the preform, suitable tools are placed on the part, the part is bagged, and then placed in an autoclave to melt and infuse the resin into the preform.

[0088] The matrix resin used for impregnating or potting the preforms described herein is a curable resin. In this disclosure, "curing" refers to the hardening of a polymer material through the chemical crosslinking of polymer chains. The term "curable" in relation to a composition means that the composition can withstand conditions that will cause the composition to reach a hardened or thermosetting state. The matrix resin is typically a curable or thermosetting resin comprising one or more uncured thermosetting or thermoplastic resins. Suitable thermosetting resins include, but are not limited to, epoxy resins, oxetanes, imides (such as polyimides or bismaleimides), vinyl ester resins, cyanate ester resins, isocyanate-modified epoxy resins, phenolic resins, furan resins, benzoxazine, formaldehyde condensation resins (such as those with urea, melamine, or phenol), polyesters, acrylic resins, mixtures therewith, blends, and combinations thereof. Suitable thermoplastic resins include, but are not limited to, polyolefins, fluoropolymers, perfluorosulfonic acids, polyamide-imides, polyamides, polyesters, polyketides, polyphenylene sulfides, polyvinylidene chloride, sulfone polymers, their hybrids, their blends, and combinations thereof.

[0089] Suitable epoxy resins include glycidyl derivatives of aromatic diamines, aromatic monoamines, aminophenols, polyphenols, polyols, and polycarboxylic acids, and non-glycidyl resins produced by the peroxidation of olefin double bonds. Examples of suitable epoxy resins include polyglycidyl ethers of bisphenols such as bisphenol A, bisphenol F, bisphenol S, bisphenol K, and bisphenol Z; polyglycidyl ethers of cresol and phenolic phenolic varnishes; glycidyl ethers of phenolic adducts; glycidyl ethers of aliphatic diols; diglycidyl ethers; diethylene glycol diglycidyl ethers; aromatic epoxy resins; aliphatic polyglycidyl ethers; epoxidized olefins; brominated resins; aromatic glycidyl amines; heterocyclic glycidyl imides and amides; glycidyl ethers; fluorinated epoxy resins; or combinations thereof.

[0090] Specific examples include tetraglycidyl derivatives of 4,4'-diaminodiphenylmethane (TGDDM), resorcinol diglycidyl ether, triglycidyl-p-aminophenol, triglycidyl-m-aminophenol, bromobisphenol F diglycidyl ether, tetraglycidyl derivatives of diaminodiphenylmethane, trihydroxyphenylmethane triglycidyl ether, polyglycidyl ether of phenol-formaldehyde phenolic varnish, polyglycidyl ether of o-cresol phenolic varnish, or tetraglycidyl ether of tetraphenylethane.

[0091] Suitable oxetane compounds are those containing at least one oxetane group per molecule, including compounds such as 3-ethyl-3-[[(3-ethyloxetane-3-yl)methoxy]methyl]oxetane, oxetane-3-methanol, 3,3-bis-(hydroxymethyl)oxetane, 3-butyl-3-methyloxetane, 3-methyl-3-oxetanemethanol, 3,3-dipropyloxetane, and 3-ethyl-3-(hydroxymethyl)oxetane.

[0092] The curable matrix resin may optionally contain one or more additives, such as curing agents, curing catalysts, comonomers, rheology control agents, tackifiers, inorganic or organic fillers, thermoplastic and / or elastomeric polymers as toughening agents, stabilizers, inhibitors, pigments, dyes, flame retardants, reactive diluents, UV absorbers, and other additives known to those skilled in the art for modifying the properties of the matrix resin before and / or after curing.

[0093] Examples of suitable curing agents include, but are not limited to, aromatic, aliphatic, and alicyclic amines, or guanidine derivatives. Suitable aromatic amines include 4,4'-diaminodiphenyl sulfone (4,4'-DDS), 3,3'-diaminodiphenyl sulfone (3,3'-DDS), 1,3-diaminobenzene, 1,4-diaminobenzene, 4,4'-diaminodiphenylmethane, and phenylenediamine (BDA); suitable aliphatic amines include ethylenediamine (EDA), 4,4'-methylenebis(2,6-diethylaniline) (M-DEA), m-xylenediamine (mXDA), diethylenetriamine (DETA), triethylenetetramine (TETA), trioxanetridecanediamine (TTDA), polyoxypropylenediamine, and other homologs. Compounds; alicyclic amines, such as diaminocyclohexane (DACH), isophorone diamine (IPDA), 4,4'-diaminodicyclohexylmethane (PACM), bis(aminopropyl)piperazine (BAPP), N-aminoethylpiperazine (N-AEP); other suitable curing agents include acid anhydrides, typically polycarboxylic acid anhydrides, such as nadic anhydride, methyl nadic anhydride, phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylene-tetrahydrophthalic anhydride, pyromellitic dianhydride, chloroendic anhydride, and trimellitic anhydride.

[0094] Other curing agents are Lewis acid: Lewis base complexes. Suitable Lewis acid: Lewis base complexes include, for example, complexes of the following: BCl3:amine complexes; BF3:amine complexes, such as BF3:monoethylamine, BF3:propylamine, BF3:isopropylamine, BF3:benzylamine, BF3:chlorobenzylamine, BF3:trimethylamine, BF3:pyridine, BF3:THF; AlCl3:THF; AlCl3:acetonitrile; and ZnCl2:THF.

[0095] Additional curing agents include polyamides, polyamines, amide-based amines, polyamide-based amines, alicyclic compounds, polyetheramides, imidazoles, dicyandiamides, substituted ureas and urea-ketones, hydrazines, and silicones.

[0096] Urea-based curing agents are a range of materials available under the trade name DYHARD (sold by Alzchem), as well as urea derivatives, such as those commercially available as UR200, UR300, UR400, UR600, and UR700. Urea-ketone accelerators include, for example, 4,4-methylenediphenyl bis(N,N-dimethylurea) (available from Onmicure as U52 M).

[0097] When a curing agent is present, the total amount of the curing agent ranges from 1 wt% to 60 wt% of the resin composition. Typically, the curing agent is present in the range of 15 wt% to 50 wt%, more typically in the range of 20 wt% to 30 wt%.

[0098] Suitable toughening agents may include, but are not limited to, homopolymers or copolymers alone or in combination with the following: polyamides, copolyamides, polyimides, aromatic polyamides, polyketides, polyetherimides (PEI), polyetherketones (PEK), polyetherketoneketones (PEKK), polyetheretherketones (PEEK), polyethersulfones (PES), polyetherethersulfones (PEES), polyesters, polyurethanes, polysulfones, polysulfides, polyphenylene oxide (PPO) and modified PPO, poly(ethylene oxide) (PEO) and polypropylene oxide, polystyrene, polybutadiene, polyacrylates, polystyrene, polymethyl methacrylates, polyacrylates, polyphenylene sulfones, high-performance hydrocarbon polymers, liquid crystal polymers, elastomers, segmental elastomers and core-shell particles.

[0099] When toughening particles or toughening agents are present, they may be present in the range of 0.1 wt% to 30 wt% of the resin composition. In one embodiment, the toughening particles or toughening agents may be present in the range of 10 wt% to 25 wt%. In another embodiment, the toughening particles or toughening agents may be present in the range of 0.1 to 10 wt%. Suitable toughening particles or toughening agents include, for example, Virantage VW10200 FRP, VW10300 FP, and VW10700 FRP from Solvay, BASF Ultrason E2020, and Sumikaexcel 5003P from Sumitomo Chemicals.

[0100] The toughening particles or toughening agents can be in the form of particles with a diameter greater than 20 micrometers to prevent them from binding into the fiber layer. The size of the toughening particles or toughening agents can be selected so that they are not filtered by the fiber reinforcement material. Optionally, the composition may also include inorganic ceramic particles, microspheres, microspheres, and clay.

[0101] The resin composition may also contain conductive particles, such as those described in PCT International Publications WO 2013 / 141916, WO 2015 / 130368 and WO 2016 / 048885.

[0102] The mold used for resin infusion can be a two-component closed mold or a vacuum-sealed single-sided mold. After the matrix resin is poured into the mold, the mold is heated to cure the resin.

[0103] During heating, the resin reacts with itself to form crosslinks within the matrix of the composite material. After an initial heating period, the resin gels. After gelation, the resin no longer flows but becomes solid. Following gelation, the temperature or curing temperature can be gradually increased to a final temperature to complete curing. The final curing temperature depends on the properties and characteristics of the selected thermosetting resin. Therefore, in a suitable method, the composite material is heated to a first temperature suitable for gelling the matrix resin, and then the temperature is gradually increased to a second temperature and held at that second temperature for a certain period to complete curing.

[0104] Therefore, composite articles are obtained by curing the composite material described herein.

[0105] The apparatus, system, method, and process disclosed herein are further illustrated by the following non-limiting examples.

[0106] Example 1. Spinning of polymer spinning solution

[0107] Polymer spinning solutions containing polyacrylonitrile-based polymers were wet-spun into a coagulation bath containing 50 / 50 DMSO / water using 50K spinnerets fixed in four different spinneret housings. The dimensions of a truncated conical shroud were varied within the spinneret housings, specifically the shroud length, the shroud opening diameter, the shroud top angle, and the shroud bottom angle. For comparison, the same polymer spinning solution containing polyacrylonitrile-based polymers was wet-spun into a coagulation bath containing 50 / 50 DMSO / water using 50K spinnerets without the spinneret housings. White fiber bundles produced with and without the spinneret housings were collected. The dimensions of the spinneret housings of this invention are summarized below.

[0108] Table 1.

[0109]

[0110] *Self-dried head measurement

[0111] The filament diameter and roundness of the fiber bundles with and without the spinneret housing of Design 2 were measured, including the variability of filament diameter and roundness.

[0112] Figure 4 The diagram shows the filament diameters of white fiber bundles manufactured using and without the spinneret housing of Design 2, including standard deviations. It is evident that the filament diameter variation of white fiber bundles manufactured using the spinneret housing of the present invention is smaller than that of white fiber bundles manufactured without the spinneret housing of the present invention, i.e., more uniform.

[0113] Figure 5 The diagram shows the roundness of white fiber bundles manufactured using and without the spinneret housing of Design 2. The roundness variation of the white fiber bundles manufactured using the spinneret housing of the present invention is less than that of the white fiber bundles manufactured without the spinneret housing of the present invention, i.e., they are more uniform.

Claims

1. A system for producing polymer fibers, the system comprising: a) A spinneret housing, the spinneret housing comprising: The main body has a hollow interior and a rear cover. A flanged cylindrical wall extending from the body, wherein the flange protrudes radially inward at the distal portion of the wall. A cylindrical tube surrounding the entire body, wherein the cylindrical tube is coaxial with the flanged cylindrical wall and has a diameter larger than that of the flanged cylindrical wall, and A fairing extending from the cylindrical tube, wherein the fairing extends beyond the distal end of the flanged cylindrical wall. b) Polymer spinning solution supply line, c) A spinneret or spinneret assembly positioned within the hollow interior of the main body, and d) A coagulation bath containing coagulation liquid. The main body, together with the flanged cylindrical wall, is entirely located within the space defined by the cylindrical tube and the rear cover, and The cylindrical tube and the body are configured such that one or more openings are present, which allow the coagulated liquid to flow through and around the spinneret or spinneret assembly.

2. The system according to claim 1, wherein, The fairing has a cylindrical shape, a truncated conical shape, or a combination thereof.

3. The system according to claim 1, wherein, The fairing has a truncated conical shape.

4. The system according to claim 3, wherein, The truncated cone shape can be symmetrical or asymmetrical.

5. The system according to any one of claims 1-3, wherein, The length of the fairing, measured from the face of the flanged cylindrical wall to the far end opening, is 10 to 100 mm.

6. The system according to claim 5, wherein, The length of the fairing, measured from the face of the flanged cylindrical wall to the far end opening, is 15 to 40 mm.

7. The system according to any one of claims 1-3, wherein, The diameter of the far-end opening of the fairing is 100 to 200 mm.

8. The system according to claim 7, wherein, The diameter of the far-end opening of the fairing is 150 to 190 mm.

9. The system according to claim 8, wherein, The diameter of the far-end opening of the fairing is 160 to 190 mm.

10. The system according to any one of claims 1-3, wherein, The spinneret housing is a combination of two or more parts that are detachably fixed together.

11. The system according to any one of claims 1-3, wherein, The fairing is removable.

12. The system according to any one of claims 1-3, wherein, The spinneret or spinneret assembly is detachably secured within the spinneret housing.

13. The system according to any one of claims 1-3, wherein, The polymer spinning solution supply line is connected to the inlet of the spinneret.

14. A method for producing polymer fibers, the method comprising: a') Provide a system according to any one of claims 1-13; as well as b') The polymer spinning solution is spun into the coagulation bath, and the polymer spinning solution is supplied to the spinneret or spinneret assembly through the polymer spinning solution supply line. During the spinning process, the coagulated liquid flows through the spinneret or spinneret assembly and flows around it.

15. The method according to claim 14, wherein, Compared to methods where the spinneret housing is absent, the variability in filament diameter and / or roundness is reduced by 5% to 50%.

16. The method according to claim 15, wherein, Compared to methods without the spinneret housing, the variability in filament diameter and / or roundness is reduced by 10% to 40%.

17. The method according to claim 16, wherein, Compared to methods without the spinneret housing, the variability in filament diameter and / or roundness is reduced by 20% to 25%.

18. A method for producing carbon fiber, the method comprising: (i) Producing polymer fibers by any one of claims 14-17; (ii) The polymer fiber produced in step (i) is oxidized to form a stable carbon fiber precursor fiber and then the stable carbon fiber precursor fiber is carbonized to produce the carbon fiber.

Citation Information

Patent Citations

  • Composite materials comprising conductive NANO-fillers

    WO2013141916A2

  • Composite materials with electrically conductive and delamination resistant properties

    WO2015130368A2

  • Composite materials with high z-direction electrical conductivity

    WO2016048885A1

  • Method for producing acrylonitrile-based fiber bundle and method for producing carbon fiber bundle

    JP2017172081A

  • Method and apparatus for spinning synthetic shapes

    US2416291A