A nitrogen-sulfur co-doped carbon-based metal-free catalyst, a preparation method and application thereof
By preparing a nitrogen-sulfur dual-doped carbon-based metal-free catalyst, the problems of metal leaching and active site poisoning in the selective hydrogenation of quinoline were solved, achieving efficient and environmentally friendly quinoline conversion and selectivity for 1,2,3,4-tetrahydroquinoline, which is suitable for the selective hydrogenation reaction of quinoline and its derivatives.
Patent Information
- Application Number
- CN202410536432.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-30
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-04-30
AI Technical Summary
Existing quinoline selective hydrogenation catalysts suffer from metal leaching problems, and the active centers of noble metal catalysts are easily poisoned in the presence of quinoline, making them difficult to use in industrial applications, especially in the biological and electronic fields where they have a fatal impact on product safety and performance.
A nitrogen-sulfur dual-doped carbon-based metal-free catalyst was prepared by using inexpensive and readily available chitin as the carbon source and thiourea as the sulfur source. The synergistic effect of nitrogen and sulfur was utilized to enhance catalytic activity and avoid contamination introduced by metals.
High conversion and selectivity were achieved in the selective hydrogenation reaction of quinoline, with a quinoline conversion rate of 91.4% and a selectivity of 93.6% for 1,2,3,4-tetrahydroquinoline. Furthermore, the catalyst can be reused, which meets the environmental protection requirements of green development.
Smart Images

Figure CN118341464B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal-free catalyst technology, specifically relating to a nitrogen-sulfur dual-doped carbon-based metal-free catalyst, its preparation method, and its application. Background Technology
[0002] N-Heterocyclic compounds are biologically active compounds, accounting for approximately 60% of all pharmaceutical substances and playing a vital role in pharmaceutical and chemical production. 1,2,3,4-Tetrahydroquinoline, as an important key intermediate, is widely used in medicine, pesticides, alkaloids, and other fields, showing great application potential. Specifically, well-known prescription drugs such as clomiphene, oxamniquinet, nicarphene, and diclofenac all contain 1,2,3,4-tetrahydroquinoline structural units. Currently, methods for synthesizing 1,2,3,4-tetrahydroquinoline include the Beckmann rearrangement, catalytic cyclization, and selective hydrogenation of N-heterocyclic compounds. Among these synthetic methods, selective hydrogenation of N-heterocyclic compounds has the advantages of fewer reaction steps and higher atom utilization, making it the simplest and most efficient method. 1,2,3,4-tetrahydroquinoline can be conveniently synthesized through the selective hydrogenation of quinoline compounds.
[0003] Currently, research on catalysts for the selective hydrogenation of quinolines and their derivatives mainly falls into two categories: homogeneous and heterogeneous. Homogeneous catalysts were the earliest studied type; however, their difficulty in separating them from the reaction system significantly limits their large-scale industrial applications. In contrast, metal-based heterogeneous catalysts are easily separated from the reaction system and reused, playing a crucial role in the chemical industry. Although metal-based catalysts have achieved promising results, metal leaching is inevitable during long-term use. For many fine chemicals used in the biological and electronic fields, even trace amounts of metal impurities can have a fatal impact on product safety and performance. In addition, the catalyst also faces the problem of being poisoned by the raw materials or products in the presence of quinoline. The literature (Journal of the American Chemical Society.2012,134(42):17592-17598) reported the use of TiO2-supported noble metal catalysts such as Pd, Pt, and Ru for the selective hydrogenation of quinoline, which proved that nitrogen atoms in quinoline and 1,2,3,4-tetrahydroquinoline can poison the active center of the metal catalyst, thereby significantly reducing the activity of the catalyst.
[0004] Metal-free catalysts, lacking metal active centers, fundamentally solve the aforementioned problems. Furthermore, they offer significant advantages such as low cost and environmental friendliness, making them ideal alternatives to metal catalysts. In recent years, carbon materials have seen rapid development in the field of catalysis due to their excellent physicochemical properties. Heteroatom doping strategies can significantly enhance the catalytic performance of carbon materials. Nitrogen atoms, with atomic radii similar to carbon atoms, can be easily incorporated into the carbon framework. Moreover, due to the difference in electronegativity, the electron distribution around carbon atoms can be significantly modulated. As the most common strategy for improving the electronic structure and physicochemical properties of carbon materials, nitrogen-doped carbon materials have received widespread attention. However, there are currently no reports of using a nitrogen-sulfur dual-doped carbon-based metal-free catalyst to catalyze the hydrogenation of quinoline to 1,2,3,4-tetrahydroquinoline. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a nitrogen-sulfur dual-doped carbon-based metal-free catalyst.
[0006] The second objective of this invention is to provide a method for preparing a nitrogen-sulfur dual-doped carbon-based metal-free catalyst.
[0007] The third objective of this invention is to provide an application of a nitrogen-sulfur dual-doped carbon-based metal-free catalyst in the selective hydrogenation reaction of quinoline.
[0008] The technical solution of this invention is summarized as follows:
[0009] A method for preparing a nitrogen-sulfur dual-doped carbon-based metal-free catalyst includes the following steps:
[0010] 1) Dissolve the sulfur-containing precursor in deionized water to obtain solution 1, and disperse chitin in anhydrous ethanol to prepare dispersion 1 with a concentration of 0.05 g / mL;
[0011] 2) Add the solution 1 dropwise into the dispersion 1 to obtain a mixture. The mass ratio of the sulfur-containing precursor to chitin is (0.5-1.5):2.5. Reflux for 2-6 hours, rotary evaporate, dry, and grind to obtain a powdered intermediate.
[0012] 3) The intermediate is subjected to programmed temperature pyrolysis in argon to obtain a nitrogen-sulfur dual-doped carbon-based metal-free catalyst.
[0013] The preferred sulfur-containing precursors are thiourea, dimethyl sulfoxide, or trithiocyanate.
[0014] The drying temperature is 60-100℃, and the drying time is 4-8 hours.
[0015] The argon gas is introduced at a rate of 10-20 mL / min.
[0016] The temperature rise rate of the programmed temperature rise is 2.5℃ / min, the pyrolysis temperature is 700-1000℃, and the pyrolysis time is 2 hours.
[0017] A nitrogen-sulfur dual-doped carbon-based metal-free catalyst prepared by any of the above preparation methods.
[0018] The above-mentioned application of a nitrogen-sulfur dual-doped carbon-based metal-free catalyst in the selective hydrogenation reaction of quinoline.
[0019] The application includes the following steps:
[0020] 1) Add the above-mentioned nitrogen-sulfur dual-doped carbon-based metal-free catalyst and quinoline to a high-pressure reactor, add solvent, introduce hydrogen gas, stir at 180-200℃, and react for 8-12 hours.
[0021] 2) Cool to room temperature, release pressure, and filter; separate the solid and filtrate, the filtrate being 1,2,3,4-tetrahydroquinoline; wash the solid sequentially with deionized water and anhydrous ethanol, and vacuum dry to obtain a nitrogen-sulfur dual-doped carbon-based metal-free catalyst, which can be reused.
[0022] The filtrate was analyzed by gas chromatography to obtain the conversion rate of quinoline and the selectivity of 1,2,3,4-tetrahydroquinoline.
[0023] The ratio of nitrogen-sulfur dual-doped carbon-based metal-free catalyst to quinoline was 20 mg: 0.25 mmol.
[0024] The solvent is deionized water, n-hexane, or toluene.
[0025] Advantages of this invention:
[0026] (1) The method of the present invention uses inexpensive and readily available nitrogen-containing biomass chitin as carbon and nitrogen source, and sulfur-containing precursor as sulfur source to prepare a nitrogen-sulfur dual-doped carbon-based metal-free catalyst. Nitrogen and sulfur elements are uniformly distributed in the carbon material, and the two work synergistically to improve the catalytic activity of the carbon material in the selective hydrogenation of quinoline.
[0027] (2) The catalyst preparation process in this invention is simple, without complicated steps, and there is no dangerous or toxic intermediate treatment process, which is in line with the current trend of green development. The prepared nitrogen and sulfur doped carbon-based metal-free catalyst is applied to the selective hydrogenation reaction of quinoline and its derivatives without the introduction of metal and acid-base additives, avoiding the pollution of products caused by metal leaching and the problem of subsequent product purification.
[0028] (3) The nitrogen-sulfur dual-doped carbon-based metalless catalyst prepared exhibits good catalytic effect in the selective hydrogenation reaction of quinoline, with a quinoline conversion rate of over 91.4% and a selectivity of over 93.6% for 1,2,3,4-tetrahydroquinoline. Attached Figure Description
[0029] Figure 1 The image shows the morphology of the nitrogen-sulfur dual-doped carbon-based metal-free catalyst prepared in Example 1.
[0030] Figure 2 XRD patterns of nitrogen-sulfur dual-doped carbon-based metal-free catalysts prepared at different pyrolysis temperatures.
[0031] Figure 3 Raman diagrams of nitrogen-sulfur dual-doped carbon-based metal-free catalysts prepared at different pyrolysis temperatures. Detailed Implementation
[0032] The present invention will be further described below with reference to embodiments.
[0033] The following embodiments will enable those skilled in the art to better understand the present invention. However, the descriptions in the embodiments are for illustrative purposes only and are not intended to limit the scope of the invention in any way.
[0034] Example 1
[0035] A method for preparing a nitrogen-sulfur dual-doped carbon-based metal-free catalyst includes the following steps:
[0036] 1) Dissolve 0.5g of thiourea in 10mL of deionized water to obtain solution 1, and disperse 2.5g of chitin in 50mL of anhydrous ethanol to prepare dispersion 1 with a concentration of 0.05g / mL;
[0037] 2) Add solution 1 dropwise into dispersion 1 to obtain a mixture with a mass ratio of thiourea to chitin of 0.5:2.5. Reflux for 2 hours, rotary evaporate, dry at 60°C for 8 hours, and grind for 30 minutes to obtain a powdered intermediate.
[0038] 3) The intermediate was subjected to programmed temperature pyrolysis in argon gas at a rate of 20 mL / min, a temperature ramp rate of 2.5 °C / min, a pyrolysis temperature of 900 °C, and a pyrolysis time of 2 hours to obtain a nitrogen-sulfur dual-doped carbon-based metal-free catalyst, denoted as SNC-900.
[0039] Example 2
[0040] A method for preparing a nitrogen-sulfur dual-doped carbon-based metal-free catalyst includes the following steps:
[0041] 1) Dissolve 1g of dimethyl sulfoxide in 10mL of deionized water to obtain solution 1, and disperse 2.5g of chitin in 50mL of anhydrous ethanol to prepare dispersion 1 with a concentration of 0.05g / mL;
[0042] 2) Add solution 1 dropwise into dispersion 1 to obtain a mixture with a mass ratio of dimethyl sulfoxide to chitin of 1:2.5. Reflux for 4 hours, rotary evaporate, dry at 80°C for 6 hours, and grind for 30 minutes to obtain a powdered intermediate.
[0043] 3) The intermediate was subjected to programmed temperature pyrolysis in argon gas at a rate of 10 mL / min, a temperature ramp rate of 2.5 °C / min, a pyrolysis temperature of 700 °C, and a pyrolysis time of 2 hours to obtain a nitrogen-sulfur dual-doped carbon-based metal-free catalyst, denoted as SNC-700.
[0044] By replacing the 700℃ in this embodiment with a pyrolysis temperature of 800℃, and keeping everything else the same as in this embodiment, a nitrogen-sulfur dual-doped carbon-based metal-free catalyst was obtained, denoted as SNC-800.
[0045] Example 3
[0046] A method for preparing a nitrogen-sulfur dual-doped carbon-based metal-free catalyst includes the following steps:
[0047] 1) Dissolve 1.5g of trithiocyanate in 10mL of deionized water to obtain solution 1, and disperse 2.5g of chitin in 50mL of anhydrous ethanol to prepare dispersion 1 with a concentration of 0.05g / mL;
[0048] 2) Add solution 1 dropwise into dispersion 1 to obtain a mixture with a mass ratio of trithiocyanate to chitin of 1.5:2.5. Reflux for 6 hours, rotary evaporate, dry at 100℃ for 4 hours, and grind for 30 minutes to obtain a powdered intermediate.
[0049] 3) The intermediate was subjected to programmed temperature pyrolysis in argon gas at a rate of 15 mL / min, a temperature ramp rate of 2.5 °C / min, a pyrolysis temperature of 1000 °C, and a pyrolysis time of 2 hours to obtain a nitrogen-sulfur dual-doped carbon-based metal-free catalyst, denoted as SNC-1000.
[0050] The obtained nitrogen-sulfur dual-doped carbon-based metal-free catalyst was characterized in a series of ways.
[0051] Figure 1 The figures show the morphological characterization of the nitrogen-sulfur dual-doped carbon-based metal-free catalyst prepared in Example 1. In (a) and (b), the prepared SNC-900 has a layered morphology and a porous surface. In (c) and (d), many short-range ordered lattice fringes are observed, indicating that the prepared catalyst contains a large number of small-sized graphene fragments. The elemental distribution image in (e) shows that nitrogen and sulfur atoms are uniformly distributed in the carbon layer, proving the success of the dual-doping strategy.
[0052] Figure 2The XRD patterns of the nitrogen-sulfur dual-doped carbon-based metal-free catalysts prepared in Examples 1 to 3 are shown. Characteristic peaks belonging to the (002) and (100) crystal planes of graphite carbon appear at 24° and 43°. The characteristic peaks are broad peaks with low intensity, indicating that crystalline and amorphous structures coexist in the material.
[0053] Figure 3 The image shows the Raman spectra of the nitrogen-sulfur dual-doped carbon-based metal-free catalysts prepared in Examples 1-3. The prepared catalysts showed a Raman spectrum at 1353 cm⁻¹. -1 D-band at 1586cm -1 There are obvious characteristic peaks at the G-band of each location, which can be observed through I... D / I G The ratio of I to γ was used to study the defect concentration and graphitization degree of the prepared nitrogen-sulfur dual-doped carbon-based metal-free catalyst. The pyrolysis temperature was increased from 700℃ to 1000℃. D / I G The values are similar.
[0054] Comparative Example 1
[0055] The only difference between this comparative example and Example 1 is that: in step 1), solution 1 is not prepared, and in step 2), solution 1 is not added, that is, no sulfur-containing precursor is added. Chitosan is directly dispersed in a mixed solution of ethanol and water. Otherwise, it is the same as Example 1, and a nitrogen-doped carbon-based metal-free catalyst is obtained.
[0056] Comparative Example 2
[0057] The only difference between this comparative example and Example 1 is that: in step (1), solution 1 is not prepared, and chitin is replaced with cellulose and dispersed in a mixed solution of ethanol and water. Otherwise, it is the same as Example 1, and a carbon catalyst without heteroatoms is prepared.
[0058] Comparative Example 3
[0059] The only difference between this comparative example and Example 1 is that in step (1), chitin is replaced with cellulose, and the rest is the same as in Example 1, to prepare a sulfur-doped carbon-based metal-free catalyst.
[0060] Example 4
[0061] The application of nitrogen-sulfur dual-doped carbon-based metal-free catalysts in the selective hydrogenation reaction of quinoline includes the following steps:
[0062] 1) 20 mg of a nitrogen-sulfur dual-doped carbon-based metal-free catalyst prepared in Example 1 and 0.25 mmol of quinoline were added to a high-pressure reactor, 3 mL of deionized water was added, and 1 MPa hydrogen gas was repeatedly introduced 10 times to purge the air in the high-pressure reactor. Then 2 MPa hydrogen gas was introduced, and the reactor was stirred at 200 °C for 8 hours.
[0063] 2) Cool to room temperature, release pressure, and filter; separate the solid and filtrate, the filtrate containing 1,2,3,4-tetrahydroquinoline; wash the solid sequentially with deionized water and anhydrous ethanol, and vacuum dry to obtain a nitrogen-sulfur dual-doped carbon-based metal-free catalyst, which can be reused.
[0064] Example 5
[0065] The application of nitrogen-sulfur dual-doped carbon-based metal-free catalysts in the selective hydrogenation reaction of quinoline includes the following steps:
[0066] 1) 20 mg of a nitrogen-sulfur dual-doped carbon-based metal-free catalyst prepared in Example 2 and 0.25 mmol of quinoline were added to a high-pressure reactor, 3 mL of n-hexane was added, and 1 MPa of hydrogen gas was repeatedly introduced 10 times to purge the air in the high-pressure reactor. Then 2 MPa of hydrogen gas was introduced, and the reactor was stirred at 190 °C for 10 hours.
[0067] 2) Cool to room temperature, release pressure, and filter; separate the solid and filtrate, the filtrate containing 1,2,3,4-tetrahydroquinoline; wash the solid sequentially with deionized water and anhydrous ethanol, and vacuum dry to obtain a nitrogen-sulfur dual-doped carbon-based metal-free catalyst, which can be reused.
[0068] Example 6
[0069] The application of nitrogen-sulfur dual-doped carbon-based metal-free catalysts in the selective hydrogenation reaction of quinoline includes the following steps:
[0070] 1) 20 mg of a nitrogen-sulfur dual-doped carbon-based metal-free catalyst prepared in Example 3 and 0.25 mmol of quinoline were added to a high-pressure reactor, 3 mL of toluene was added, and 1 MPa of hydrogen gas was repeatedly introduced 10 times to purge the air in the high-pressure reactor. Then 2 MPa of hydrogen gas was introduced, and the reactor was stirred at 180 °C for 12 hours.
[0071] 2) Cool to room temperature, release pressure, and filter; separate the solid and filtrate, the filtrate containing 1,2,3,4-tetrahydroquinoline. Wash the solid sequentially with deionized water and anhydrous ethanol, and vacuum dry to obtain a nitrogen-sulfur dual-doped carbon-based metal-free catalyst, which can be reused.
[0072] Comparative Example 4
[0073] The application of the catalyst prepared in Comparative Example 1 in the selective hydrogenation reaction of quinoline includes the following steps: replacing the nitrogen-sulfur dual-doped carbon-based metalless catalyst prepared in Example 1 of Example 4 with 20 mg of the catalyst prepared in Comparative Example 1, and the rest is the same as in Example 4, with the filtrate containing 1,2,3,4-tetrahydroquinoline.
[0074] Comparative Example 5
[0075] The application of the catalyst prepared in Comparative Example 2 in the selective hydrogenation reaction of quinoline includes the following steps: replacing the nitrogen-sulfur dual-doped carbon-based metalless catalyst prepared in Example 1 of Example 4 with 20 mg of the catalyst prepared in Comparative Example 2, and the rest is the same as in Example 4, with the filtrate containing 1,2,3,4-tetrahydroquinoline.
[0076] Comparative Example 6
[0077] The application of the catalyst prepared in Comparative Example 3 in the selective hydrogenation reaction of quinoline includes the following steps: replacing the nitrogen-sulfur dual-doped carbon-based metalless catalyst prepared in Example 1 of Example 4 with 20 mg of the catalyst prepared in Comparative Example 3, and the rest is the same as in Example 4, with the filtrate containing 1,2,3,4-tetrahydroquinoline.
[0078] Table 1 shows the catalytic effects of catalysts prepared in different examples or comparative examples in the selective hydrogenation reaction of quinoline.
[0079] Table 1
[0080]
[0081] The blank control follows the steps of Example 4, but without the nitrogen-sulfur dual-doped carbon-based metal-free catalyst prepared in Example 1.
Claims
1. The application of a nitrogen-sulfur dual-doped carbon-based metal-free catalyst in the selective hydrogenation reaction of quinoline, characterized in that... Includes the following steps: 1) Add the nitrogen-sulfur dual-doped carbon-based metal-free catalyst and quinoline to a high-pressure reactor, add solvent, introduce hydrogen gas, stir at 180-200℃, and react for 8-12 hours. 2) Cool to room temperature, release pressure, and filter; separate the solid and filtrate, the filtrate being 1,2,3,4-tetrahydroquinoline; wash the solid sequentially with deionized water and anhydrous ethanol, and vacuum dry; the obtained nitrogen-sulfur dual-doped carbon-based metal-free catalyst can be reused. The preparation method of the nitrogen-sulfur dual-doped carbon-based metal-free catalyst includes the following steps: A dissolves a sulfur-containing precursor in deionized water to obtain solution 1, and disperses chitin in anhydrous ethanol to prepare dispersion 1; the sulfur-containing precursor is thiourea, dimethyl sulfoxide, or trithiocyanate. B. The solution 1 is added dropwise to the dispersion 1 to obtain a mixture. The mass ratio of the sulfur-containing precursor to chitin is (0.5~1.5):2.
5. The mixture is refluxed for 2-6 hours, rotary evaporated, dried, and ground to obtain a powdered intermediate. The drying temperature is 60-100℃ and the drying time is 4-8 hours. C. The intermediate is subjected to programmed temperature pyrolysis in argon gas to obtain a nitrogen-sulfur dual-doped carbon-based metal-free catalyst; the argon gas flow rate is 10-20 mL / min; the programmed temperature rise rate is 2.5℃ / min; the pyrolysis temperature is 700-1000℃; and the pyrolysis time is 2 hours.
2. The application according to claim 1, characterized in that: The ratio of the nitrogen-sulfur dual-doped carbon-based metal-free catalyst to quinoline is 20 mg: 0.25 mmol.
3. The application according to claim 1, characterized in that: The solvent is deionized water, n-hexane, or toluene.
Citation Information
Patent Citations
Preparation and hydrogen production application of non-metal biomass-based porous carbon material
CN113233461A
Method for realizing quinoline hydrogenation by taking nitrogen-boron double-doped carbon nanomaterial as catalyst