Method for improving hot deformation performance of as-cast high-entropy alloy
By employing differential thermal analysis and hot isostatic pressing, a pretreatment method for as-cast AlCrNbMoTaTiHf high-entropy alloys was developed. This method addresses the problem of poor hot deformation performance of as-cast high-entropy alloys, improves the hot deformation performance of both ingot and laser additive high-entropy alloys, and promotes their application in hot-end components of aero-engines.
Patent Information
- Application Number
- CN202410554652.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-07
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-05-07
Smart Images

Figure CN118345321B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for improving the hot deformation properties of as-cast high-entropy alloys. This method is specifically designed for AlCrNbMoTaTiHf high-entropy alloys and belongs to the field of metallic materials technology. Background Technology
[0002] Refractory high-entropy alloys possess excellent high-temperature properties and are highly promising new high-temperature resistant structural materials. Among them, the AlCrNbMoTaTiHf refractory high-entropy alloy, composed of Al, Cr, Nb, Mo, Ta, Ti, and Hf, has suitable density, high melting point, and high-temperature performance, and is expected to replace nickel-based superalloys, becoming one of the important new high-temperature resistant candidate materials for hot-end components of advanced aero-engines.
[0003] High-melting-point AlCrNbMoTaTiHf high-entropy alloys exhibit problems such as dendritic segregation, low-melting-point phases, and inhomogeneous microstructure after melting, resulting in poor hot deformation performance and hindering subsequent billeting and forging. Pretreatment methods before hot deformation are crucial for improving the hot deformation performance of as-cast AlCrNbMoTaTiHf refractory high-entropy alloys. However, currently, there is a lack of pretreatment methods to improve the hot deformation performance of this as-cast refractory high-entropy alloy, especially for as-cast AlCrNbMoTaTiHf alloys with different compositions. Therefore, it is necessary to develop pretreatment control methods to improve the hot deformation performance of as-cast AlCrNbMoTaTiHf refractory high-entropy alloys with different compositions, thereby effectively enhancing the hot deformation capability of this high-entropy alloy and promoting its engineering applications. Summary of the Invention
[0004] This invention addresses the shortcomings of the existing technology by providing a method to improve the hot deformation performance of as-cast high-entropy alloys. This method involves pretreatment of as-cast AlCrNbMoTaTiHf high-entropy alloys before hot deformation. The purpose is to improve the hot deformation performance of as-cast AlCrNbMoTaTiHf high-entropy alloys with different compositions, accelerate the engineering application of this refractory high-entropy alloy, and meet the application requirements of new high-temperature resistant structural materials for hot-end components of next-generation aero-engines.
[0005] The objective of this invention is achieved through the following technical solution:
[0006] The method for improving the hot deformation performance of as-cast high-entropy alloys described in this invention is a pretreatment of as-cast AlCrNbMoTaTiHf high-entropy alloys before hot deformation. The steps of this method are as follows:
[0007] Step 1: Measure the phase transformation temperature of the as-cast AlCrNbMoTaTiHf high-entropy alloy.
[0008] Using a differential thermal analyzer with a heating rate of 10℃ / min, the phase transformation temperature of the as-cast AlCrNbMoTaTiHf high-entropy alloy was obtained by automatically measuring the changes in temperature and temperature difference.
[0009] Step 2: Hot isostatic pressing of the as-cast AlCrNbMoTaTiHf high-entropy alloy.
[0010] The as-cast AlCrNbMoTaTiHf high-entropy alloy was placed in a hot isostatic pressing apparatus and subjected to hot isostatic pressing treatment at 1180–1250℃ and 320–450MPa for 1–3 hours.
[0011] Step 3: Heat treatment of the as-cast AlCrNbMoTaTiHf high-entropy alloy
[0012] When the AlCrNbMoTaTiHf high-entropy alloy has only one phase transformation point, the as-cast high-entropy alloy is heated to 20°C above the phase transformation point and held for 5 to 20 hours, then furnace cooled to room temperature and removed from the furnace.
[0013] When the AlCrNbMoTaTiHf high-entropy alloy has two phase transformation points, the as-cast AlCrNbMoTaTiHf high-entropy alloy is first heated to 10-30°C above the low-temperature phase transformation point and held for 3-15 hours. Then, the as-cast AlCrNbMoTaTiHf high-entropy alloy is heated to 20°C above the high-temperature phase transformation point and held for 10-30 hours. After that, it is furnace cooled to room temperature and removed from the furnace.
[0014] In addition, the chemical composition and molar percentage of the as-cast AlCrNbMoTaTiHf high-entropy alloy are as follows: Al 2%–8%, Cr 2%–6%, Nb 18%–28%, Mo 4%–10%, Ta 6%–10%, Ti 16%–52%, and Hf 16%–22%.
[0015] Furthermore, the chemical composition and molar percentage of the as-cast AlCrNbMoTaTiHf high-entropy alloy are as follows: Al 4%, Cr 4%, Nb 18%, Mo 8%, Ta 12%, Ti 34%, Hf 20%.
[0016] In addition, in step two, the as-cast AlCrNbMoTaTiHf high-entropy alloy is hot isostatically pressed and then slowly cooled to 500°C in the furnace before being removed from the furnace and air-cooled.
[0017] In addition, in step three, the heating rate of the as-cast AlCrNbMoTaTiHf high-entropy alloy is 100–300 °C / h.
[0018] The technical solution of this invention is characterized by:
[0019] Since cast high-entropy alloys are prone to defects such as porosity, they are likely to form crack sources during hot deformation, leading to a decrease in hot deformation performance. Hot isostatic pressing can effectively close internal defects in cast high-entropy alloys. Therefore, the technical solution of this invention first utilizes hot isostatic pressing to improve the hot deformation performance of cast AlCrNbMoTaTiHf high-entropy alloys.
[0020] Phase structure and microstructure also significantly influence the hot deformation properties of as-cast AlCrNbMoTaTiHf high-entropy alloys. For example, when low-melting-point phases are present in as-cast AlCrNbMoTaTiHf high-entropy alloys, these phases melt first during heating, forming crack initiation sites and thus reducing the hot deformation properties of the as-cast high-entropy alloys. Dendritic segregation also reduces the hot deformation properties of as-cast AlCrNbMoTaTiHf high-entropy alloys, and studies have shown that dendritic segregation gradually improves when the heating temperature exceeds 20°C above the high-temperature phase transformation point.
[0021] High-entropy alloys have a large compositional space. Some as-cast AlCrNbMoTaTiHf high-entropy alloys do not have low-melting-point phases and do not require remelting heat treatment at the low-temperature phase transformation point. They only need pretreatment control at a temperature 20°C above the high-temperature phase transformation point. Therefore, the technical solution of this invention determines the phase transformation point of the as-cast high-entropy alloy using differential thermal analysis and then adopts different pretreatment control methods according to different types of phase transformation points to improve the hot deformation performance of the as-cast high-entropy alloy.
[0022] Based on the above-mentioned features of the technical solution of the present invention, the beneficial effects it produces are as follows:
[0023] 1. Hot isostatic pressing can effectively close internal defects in high-entropy alloy ingots, which helps reduce ingot cracking and improve the hot deformation performance of high-entropy alloys.
[0024] 2. By using differential thermal analysis to determine the phase transformation points of high-entropy alloys with different compositions of AlCrNbMoTaTiHf, different heat treatments can be applied to high-entropy alloys with different compositions to eliminate possible low-melting-point phases and improve dendrite segregation, thereby controlling the microstructure before hot deformation and effectively improving hot deformation performance.
[0025] 3. The pretreatment control method of the present invention is applicable to improving the hot deformation performance of high-entropy alloys in the molten and cast AlCrNbMoTaTiHf system, and is also applicable to the hot deformation performance of high-entropy alloys in the laser additive AlCrNbMoTaTiHf system. Attached image description:
[0026] Figure 1 Al4Cr2Nb in Example 1 20 Mo 10 Ta6Ti 38 Hf20 As-cast microstructure of the alloy
[0027] Figure 2 Al4Cr2Nb in Example 1 20 Mo 10 Ta6Ti 38 Hf 20 Microstructure of the alloy after pretreatment
[0028] Figure 3 Al4Cr4Nb in Example 2 18 Mo8Ta 12 Ti 34 Hf 20 As-cast microstructure of the alloy
[0029] Figure 4 Al4Cr4Nb in Example 2 18 Mo8Ta 12 Ti 34 Hf 20 Microstructure of the alloy after pretreatment Detailed Implementation
[0030] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments:
[0031] Example 1
[0032] In this embodiment, the molar expression for the AlCrNbMoTaTiHf high-entropy alloy is Al4Cr2Nb. 20 Mo 10 Ta6Ti 38 Hf 20 The molar percentages of each component in the expression were converted to weight percentages, and a cast AlCrNbMoTaTiHf high-entropy alloy was obtained by remelting five times using a magnetic levitation melting method. Its microstructure is as follows: Figure 1 As shown.
[0033] The pretreatment control method described in this invention is used to improve the hot deformation properties of the as-cast AlCrNbMoTaTiHf high-entropy alloy. The steps are as follows:
[0034] Step 1: Using a differential thermal analyzer, set the heating rate to 10℃ / min, and obtain the as-cast Al4Cr2Nb by automatically measuring the changes in temperature and temperature difference. 20 Mo 10 Ta6Ti 38 Hf 20 The phase transformation points of high-entropy alloys are 752℃ and 1189℃;
[0035] Step 2: Add the as-cast Al4Cr2Nb 20Mo 10 Ta6Ti 38 Hf 20 The high-entropy alloy was placed in a hot isostatic pressing apparatus and subjected to hot isostatic pressing treatment at 1220℃ and 400MPa for 1.5 hours, and then slowly cooled to 500℃ in the furnace before being removed from the furnace and air-cooled.
[0036] Step 3: Heat the as-cast Al4Cr2Nb at a heating rate of 200℃ / h. 20 Mo 10 Ta6Ti 38 Hf 20 The high-entropy alloy was heated to 775°C and held for 5 hours. Then, the cast alloy was heated to 1209°C and held for 18 hours. After that, it was furnace cooled to room temperature and removed from the furnace.
[0037] See Figure 2 After pretreatment and regulation, the as-cast Al4Cr2Nb 20 Mo 10 Ta6Ti 38 Hf 20 The high-entropy alloy microstructure has eliminated low-melting-point phases and porosity defects, with no obvious dendritic segregation and a relatively uniform microstructure.
[0038] Example 2
[0039] In this embodiment, the molar expression for the AlCrNbMoTaTiHf high-entropy alloy is Al4Cr4Nb. 18 Mo8Ta 12 Ti 34 Hf 20 The molar percentages of each component in the expression were converted to weight percentages, and a cast AlCrNbMoTaTiHf high-entropy alloy was obtained by remelting five times using a magnetic levitation melting method. Its microstructure is as follows: Figure 3 As shown.
[0040] The pretreatment control method described in this invention is used to improve the hot deformation properties of the as-cast AlCrNbMoTaTiHf high-entropy alloy. The steps are as follows:
[0041] Step 1: Using a differential thermal analyzer, set the heating rate to 10℃ / min, and obtain the as-cast Al4Cr4Nb by automatically measuring the changes in temperature and temperature difference. 18 Mo8Ta 12 Ti 34 Hf 20 The phase transformation point of the high-entropy alloy is 1215℃;
[0042] Step 2: Add the as-cast Al4Cr4Nb 18 Mo8Ta 12 Ti 34 Hf20 The high-entropy alloy was placed in a hot isostatic pressing apparatus and subjected to hot isostatic pressing treatment at 1200℃ and 350MPa for 2 hours. It was then slowly cooled to 500℃ in the furnace and then removed from the furnace and air-cooled.
[0043] Step 3: Heat the as-cast Al4Cr4Nb at a heating rate of 150℃ / h. 18 Mo8Ta 12 Ti 34 Hf 20 The high-entropy alloy was heated to 1230℃, held at that temperature for 10 hours, then cooled to room temperature and removed from the furnace.
[0044] See Figure 4 After pretreatment and regulation, the as-cast Al4Cr4Nb 18 Mo8Ta 12 Ti 34 Hf 20 The high-entropy alloy has eliminated porosity defects, has no obvious dendritic segregation, and has a relatively uniform microstructure.
[0045] Example 3
[0046] In this embodiment, the molar expression for the AlCrNbMoTaTiHf high-entropy alloy is Al4Cr6Nb. 20 Mo8Ta 10 Ti 36 Hf 16 The molar percentages of each component in the expression were converted to weight percentages, and the as-cast AlCrNbMoTaTiHf high-entropy alloy was obtained by remelting five times using the magnetic levitation melting method.
[0047] The pretreatment control method described in this invention is used to improve the hot deformation properties of the as-cast AlCrNbMoTaTiHf high-entropy alloy. The steps are as follows:
[0048] Step 1: Using a differential thermal analyzer, set the heating rate to 10℃ / min, and obtain the as-cast Al4Cr6Nb by automatically measuring the changes in temperature and temperature difference. 20 Mo8Ta 10 Ti 36 Hf 16 The phase transformation point of high-entropy alloys is 1204℃;
[0049] Step 2: Add the as-cast Al4Cr6Nb 20 Mo8Ta 10 Ti 36 Hf 16 The high-entropy alloy was placed in a hot isostatic pressing apparatus and subjected to hot isostatic pressing treatment at 1180℃ and 450MPa for 3 hours. It was then slowly cooled to 500℃ in the furnace and then removed from the furnace and air-cooled.
[0050] Step 3: Heat the as-cast Al4Cr6Nb at a heating rate of 180℃ / h. 20 Mo8Ta 10 Ti 36 Hf 16 The high-entropy alloy was heated to 1224℃, held at that temperature for 12 hours, then cooled to room temperature and removed from the furnace.
[0051] Pre-treated and regulated as-cast Al4Cr6Nb 20 Mo8Ta 10 Ti 36 Hf 16 The high-entropy alloy has eliminated porosity defects, has no obvious dendritic segregation, and has a relatively uniform microstructure.
[0052] Example 4
[0053] In this embodiment, the molar expression for the AlCrNbMoTaTiHf high-entropy alloy is Al6Cr2Nb. 28 Mo 10 Ta8Ti 26 Hf 20 The molar percentages of each component in the expression were converted to weight percentages, and the as-cast AlCrNbMoTaTiHf high-entropy alloy was obtained by remelting five times using the magnetic levitation melting method.
[0054] The pretreatment control method described in this invention is used to improve the hot deformation properties of the as-cast AlCrNbMoTaTiHf high-entropy alloy. The steps are as follows:
[0055] Step 1: Using a differential thermal analyzer, set the heating rate to 10℃ / min, and obtain the as-cast Al6Cr2Nb by automatically measuring the changes in temperature and temperature difference. 28 Mo 10 Ta8Ti 26 Hf 20 The phase transformation points of the high-entropy alloy are 969℃ and 1197℃;
[0056] Step 2: Add the as-cast Al6Cr2Nb 28 Mo 10 Ta8Ti 26 Hf 20 The high-entropy alloy was placed in a hot isostatic pressing apparatus and subjected to hot isostatic pressing treatment at 1240℃ and 450MPa for 1 hour, and then slowly cooled to 500℃ in the furnace before being removed from the furnace and air-cooled.
[0057] Step 3: Heat the as-cast Al6Cr2Nb at a heating rate of 220℃ / h. 28 Mo 10 Ta8Ti 26 Hf 20The high-entropy alloy was heated to 980°C and held for 8 hours. Then, the cast alloy was heated to 1217°C and held for 20 hours. After that, it was furnace cooled to room temperature and removed from the furnace.
[0058] As-cast Al6Cr2Nb after pretreatment and regulation 28 Mo 10 Ta8Ti 26 Hf 20 The high-entropy alloy microstructure has eliminated low-melting-point phases and porosity defects, with no obvious dendritic segregation and a relatively uniform microstructure.
Claims
1. A method for improving the hot deformation properties of as-cast high-entropy alloys, characterized in that: This method is a pretreatment for as-cast AlCrNbMoTaTiHf high-entropy alloys before hot deformation. The chemical composition and molar percentage of the as-cast AlCrNbMoTaTiHf high-entropy alloy are: Al 2%–8%, Cr 2%–6%, Nb 18%–28%, Mo 4%–10%, Ta 6%–10%, Ti 16%–52%, and Hf 16%–22%. The steps of this method are as follows: Step 1: Measure the phase transformation temperature of the as-cast AlCrNbMoTaTiHf high-entropy alloy. Using a differential thermal analyzer, the heating rate is set to 10℃ / min. The phase transformation temperature of the as-cast AlCrNbMoTaTiHf high-entropy alloy is obtained by automatically measuring the changes in temperature and temperature difference. Step 2: Hot isostatic pressing of the as-cast AlCrNbMoTaTiHf high-entropy alloy. The as-cast AlCrNbMoTaTiHf high-entropy alloy is placed in a hot isostatic pressing apparatus and subjected to hot isostatic pressing treatment at 1180~1250℃ and 320~450MPa for 1~3 hours. Step 3: Heat treatment of the as-cast AlCrNbMoTaTiHf high-entropy alloy. When the AlCrNbMoTaTiHf high-entropy alloy has only one phase transformation point, heat the as-cast high-entropy alloy to 20°C above the phase transformation point and hold for 5–20 hours, then furnace cool to room temperature and remove from the furnace. When the AlCrNbMoTaTiHf high-entropy alloy has two phase transformation points, first heat the as-cast AlCrNbMoTaTiHf high-entropy alloy to 10–30°C above the low-temperature phase transformation point and hold for 3–15 hours, then heat the as-cast AlCrNbMoTaTiHf high-entropy alloy to 20°C above the high-temperature phase transformation point, hold for 10–30 hours, then furnace cool to room temperature and remove from the furnace.
2. The method for improving the hot deformation properties of as-cast high-entropy alloys according to claim 1, characterized in that: The chemical composition and molar percentage of the as-cast AlCrNbMoTaTiHf high-entropy alloy are as follows: Al 4%, Cr 4%, Nb 18%, Mo 8%, Ta 12%, Ti 34%, Hf 20%.
3. The method for improving the hot deformation properties of as-cast high-entropy alloys according to claim 1, characterized in that: In step two, the as-cast AlCrNbMoTaTiHf high-entropy alloy is hot isostatically pressed and then slowly cooled to 500°C in the furnace before being removed from the furnace and air-cooled.
4. The method for improving the hot deformation properties of as-cast high-entropy alloys according to claim 1, characterized in that: In step three, the heating rate of the as-cast AlCrNbMoTaTiHf high-entropy alloy is 100–300 °C / h.
Citation Information
Patent Citations
High-entropy alloy forging and stamping process
CN113249630A
Blank making method of refractory high-entropy alloy cast ingot
CN114147081A