A catalyst for the oxidation of isononyl alcohol to isononanoic acid and isononyl isononanoate, its preparation method and use
By using a nitrogen-doped carbon-supported PtBi bimetallic catalyst in a high-pressure autoclave process, isononol was converted into isononanoic acid and isonononoic acid ester under mild conditions, solving the problems of harsh conditions and safety risks in existing technologies and achieving efficient and environmentally friendly catalytic effects.
Patent Information
- Application Number
- CN202410518871.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-28
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-04-28
AI Technical Summary
Existing methods for the oxidation of isononyl alcohol to prepare isononanoic acid and isononyl isononanoate have harsh reaction conditions, stability issues with homogeneous catalysts, and the use of hydrogen peroxide and homogeneous catalysts poses safety risks and environmental pollution.
Using a nitrogen-doped carbon-supported PtBi bimetallic catalyst, isononol was converted into isononanoic acid and isonononoic acid ester under mild conditions without solvent or alkali in a high-pressure autoclave process via hydrogen reduction.
The catalyst achieves highly selective conversion of isononol to isononanoic acid and isonononoic acid ester under low temperature and low pressure conditions. It exhibits excellent activity, selectivity and recyclability, and meets the requirements of green chemistry, avoiding the separation and corrosion problems in traditional methods.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of catalyst technology, specifically to a catalyst for the oxidation of isononyl alcohol to prepare isononanoic acid and isononyl isononanoate, its preparation method, and its application. Background Technology
[0002] Isonononic acid (3,5,5-trimethyl-1-hexanoic acid) is a fine chemical intermediate widely used in coatings, lubricants, plasticizers, and alkyd resin modification. It is also used to produce various isonononate esters for use in cosmetics. Traditional methods for producing isonononic acid primarily involve the oxidation of isononal. However, these methods typically require harsh reaction conditions and the addition of a homogeneous catalyst. For example, patent CN108047027A proposes a method for preparing isonononic acid by catalytic oxidation of isononal under relatively mild conditions using a metal-organic framework catalyst. While this method is relatively mild, the poor thermal stability and acid / alkali resistance of the metal-organic framework catalyst may affect its stability. Another example is the continuous oxidation process of isononal in a microchannel reactor used by Qiao Bin et al. to produce isonononic acid, achieving a yield of >95% under relatively mild reaction conditions. However, this process requires the addition of manganese acetate as a homogeneous catalyst (Fine Petrochemicals, 2023, Vol. 40, No. 5, pp. 56-69). Therefore, these processes increase the difficulty of product purification and also introduce safety risks and environmental pollution problems.
[0003] Isononanol (3,5,5-trimethyl-1-hexanol) oxidation can also directly yield isononanoic acid. Patent WO2022116243A1 proposes a one-step oxidation process using isononanol as a raw material, hydrogen peroxide solution as an oxidant, and the addition of a co-oxidant and a phase transfer catalyst under acidic conditions to prepare isononanoic acid, with an isononanoic acid yield of 65-91%. However, phase transfer catalysts such as hexadecyltrimethylammonium hydrogen sulfate are expensive, and the use of hydrogen peroxide increases the technical risk of this process. Another patent, CN112657510A, proposes a catalyst for the catalytic oxidation of isononanol to isononanoic acid, its preparation method, and its application. This method uses palladium supported by activated carbon and copper or cobalt as a co-catalyst. The catalyst is loaded by impregnation and then subjected to wet reduction. The resulting catalyst exhibits a high isononanol conversion rate and 99.9% isononanoic acid selectivity. This technology offers higher product selectivity compared to traditional methods, but it places high demands on the catalyst reaction conditions. For example, the reaction temperature is 110–120°C, the reaction atmosphere is pure oxygen, and the reaction pressure is 0.8–1.2 MPa; and sodium hydroxide needs to be added to the reaction system.
[0004] Given the limitations of existing technologies, developing a novel catalyst and its application method to efficiently convert isononanol to isononanoic acid and isonononocyanate under milder conditions is of significant research and application value. The novel catalyst should possess excellent catalytic performance, high selectivity, and environmental friendliness to meet the requirements of green chemistry and sustainable development.
[0005] This invention employs a nitrogen-doped carbon-supported PtBi bimetallic catalyst and a high-pressure autoclave process to achieve highly selective conversion of isononyl alcohol to isononanoic acid and isononyl isononanoate under mild reaction conditions with no solvent or with the addition of deionized water and no alkali. Summary of the Invention
[0006] The purpose of this invention is to provide a nitrogen-doped carbon-supported PtBi bimetallic catalyst and a high-pressure reactor process to achieve highly selective conversion of isononyl alcohol to isononanoic acid and isonononoic acid ester under mild reaction conditions without solvent or with added deionized water and without alkali. This solves the safety risks associated with the use of hydrogen peroxide in the current reaction system, as well as the problems of separation, corrosion and solid waste caused by the use of homogeneous catalysts and the addition of alkali.
[0007] To achieve the above objectives, the present invention adopts the following technical solution:
[0008] A catalyst for the oxidation of isononol to prepare isononanoic acid and isonononyl isononanoate, wherein the catalyst is a nitrogen-doped carbon-supported PtBi bimetallic catalyst (PtBi / NC catalyst) composed of three components: active component Pt, promoter Bi, and support nitrogen-doped carbon (NC).
[0009] Furthermore, the catalyst active component Pt has a mass fraction of 1-7%, the promoter Bi has a mass fraction of 1-5%, and the remainder is nitrogen-doped carbon support.
[0010] Furthermore, the nitrogen-doped carbon carrier is obtained by mechanically mixing activated carbon with a nitrogen-containing precursor and then pyrolyzing it at high temperature, wherein the nitrogen-containing precursor includes urea, cyanamide, dicyandiamide or melamine; or it is obtained by high-temperature pyrolysis of a nitrogen-containing organic polymer, wherein the nitrogen-containing organic polymer includes polyaniline or polydopamine.
[0011] Furthermore, in the case of obtaining activated carbon by mechanically mixing it with a nitrogen-containing precursor and then subjecting it to high-temperature pyrolysis, the mass ratio of the activated carbon to the nitrogen-containing precursor is 10:10-20, and the high-temperature pyrolysis conditions are treatment at 700-1000℃ for 1-24 hours under an inert atmosphere; in the case of obtaining activated carbon by high-temperature pyrolysis of nitrogen-containing organic polymers, the high-temperature pyrolysis conditions are treatment at 800-1200℃ for 6-24 hours under an inert atmosphere.
[0012] The preparation method of the above catalyst includes the following steps: dissolving Pt precursor and Bi precursor together in hydrochloric acid solution, then loading them onto a nitrogen-doped carbon support by impregnation, and then drying to obtain the catalyst.
[0013] Furthermore, the Pt precursor includes chloroplatinic acid, the Bi precursor includes BiCl3, and the hydrochloric acid solution concentration is 0.5–1.5 mol / L.
[0014] Furthermore, the drying conditions are 50–120°C for 6–24 hours.
[0015] The above-mentioned catalyst is used in the oxidation of isononol to prepare isonononic acid and isononyl isononanoate. In this process, the catalyst is first placed in a tube furnace for hydrogen reduction. After cooling to room temperature, the catalyst is loaded into a high-pressure reactor. Then, isononol and deionized water are added to the high-pressure reactor, or isononol is added to the high-pressure reactor alone. The high-pressure reactor is then continuously purged with oxygen-containing gas. The high-pressure reactor is then pressurized to the specified pressure and the temperature is raised. After reaching the reaction temperature, stirring is started to carry out the reaction.
[0016] Furthermore, the reduction conditions are as follows: hydrogen flow rate of 50–200 ml / min, reduction temperature of 300–550 °C, heating rate of 5–10 °C / min, reduction time of 1–20 h, and reduction pressure of atmospheric pressure.
[0017] Furthermore, the reaction conditions are as follows: the mass ratio of isononol to catalyst is 5–20:1, the mass ratio of deionized water to catalyst is 0–60:1, the oxygen-containing gas includes O2 or air, the O2 pressure is 0.3–0.9 MPa, the air pressure is 0.5–2.0 MPa, the reaction temperature is 40–100℃, the stirring speed is 600–1000 rpm, and the reaction time is 6–72 h.
[0018] The beneficial effects of this invention are:
[0019] The nitrogen-doped carbon-supported PtBi bimetallic catalyst (PtBi / NC catalyst) disclosed in this invention, after hydrogen reduction, achieves highly selective conversion of isononanol to isononanoic acid and isonononoic acid ester in a high-pressure autoclave process under mild reaction conditions (low temperature and low pressure) without solvent or with the addition of deionized water and without alkali. This catalyst can effectively control the selectivity of the products, preferentially obtaining isononanoic acid and its ester compounds, and exhibits excellent activity, selectivity and recyclability.
[0020] Furthermore, the entire catalytic reaction process of this invention produces few byproducts and does not require the use of alkali or other harmful organic solvents, which meets the requirements of green chemistry and solves the problems of separation, corrosion and solid waste caused by the use of homogeneous catalysts and the addition of alkali in traditional processes. Detailed Implementation
[0021] The present invention will be further explained below with reference to the embodiments. The following embodiments are for illustrative purposes only and are not intended to limit the scope of the invention.
[0022] A catalyst for the oxidation of isononol to prepare isononanoic acid and isonononyl isononanoate, wherein the catalyst is a nitrogen-doped carbon-supported PtBi bimetallic catalyst (PtBi / NC catalyst) composed of three components: active component Pt, promoter Bi, and support nitrogen-doped carbon (NC).
[0023] In some embodiments, the mass fraction of the catalyst active component Pt is 1-7%, the mass fraction of the promoter Bi is 1-5%, and the remainder is nitrogen-doped carbon support.
[0024] In some embodiments, the nitrogen-doped carbon carrier is obtained by mechanically mixing activated carbon with a nitrogen-containing precursor followed by high-temperature pyrolysis. In some embodiments, the nitrogen-containing precursor includes urea, cyanamide, dicyandiamide, or melamine. In some embodiments, the mass ratio of activated carbon to the nitrogen-containing precursor is 10:10-20. In some embodiments, the high-temperature pyrolysis conditions are treatment at 700–1000°C for 1–24 hours under an inert atmosphere.
[0025] In some embodiments, the nitrogen-doped carbon carrier is obtained by high-temperature pyrolysis of a nitrogen-containing organic polymer. In some embodiments, the nitrogen-containing organic polymer includes polyaniline or polydopamine. In some embodiments, the high-temperature pyrolysis conditions are treatment at 800–1200°C for 6–24 hours under an inert atmosphere.
[0026] The preparation method of the above catalyst includes the following steps: dissolving Pt precursor and Bi precursor together in hydrochloric acid solution, then loading them onto a nitrogen-doped carbon support by impregnation, and then drying to obtain the catalyst.
[0027] In some embodiments, the Pt precursor includes chloroplatinic acid, the Bi precursor includes BiCl3, and the hydrochloric acid solution concentration is 0.5–1.5 mol / L.
[0028] In some embodiments, the drying conditions are 50–120°C for 6–24 hours.
[0029] The above-mentioned catalyst is used in the oxidation of isononol to prepare isonononic acid and isononyl isononanoate. In this process, the catalyst is first placed in a tube furnace for hydrogen reduction. After cooling to room temperature, the catalyst is loaded into a high-pressure reactor. Then, isononol and deionized water are added to the high-pressure reactor, or isononol is added to the high-pressure reactor alone. The high-pressure reactor is then continuously purged with oxygen-containing gas. The high-pressure reactor is then pressurized to the specified pressure and the temperature is raised. After reaching the reaction temperature, stirring is started to carry out the reaction.
[0030] In some embodiments, the reduction conditions are as follows: hydrogen flow rate of 50–200 ml / min, reduction temperature of 300–550 °C, heating rate of 5–10 °C / min, reduction time of 1–20 h, and reduction pressure of atmospheric pressure.
[0031] In some embodiments, the reaction conditions are as follows: the mass ratio of isononol to catalyst is 5–20:1, the mass ratio of deionized water to catalyst is 0–60:1, the oxygen-containing gas includes O2 or air, the O2 pressure is 0.3–0.9 MPa, the air pressure is 0.5–2.0 MPa, the reaction temperature is 40–100°C, the stirring speed is 600–1000 rpm, and the reaction time is 6–72 h.
[0032] In each embodiment, the conversion rate and selectivity are calculated using the following formulas (all units of measurement are molar amounts):
[0033] Isononol conversion rate = (Isononol in feedstock - Isononol in product) / Isononol in feedstock × 100%
[0034] Isononanoic acid selectivity = (Isononanoic acid in the product) / (converted isononol) × 100%
[0035] Selectivity of isononyl isononanoate = (Isononyl isononanoate in the product x 2) / (converted isononol) x 100%
[0036] The qualitative and quantitative analysis of the raw materials and products before and after the reaction was performed on an Agilent gas chromatograph 7890, and the component analysis was carried out using an FFAP capillary column and an FID detector.
[0037] Example 1
[0038] PtBi / NC-1 catalyst: 10g of commercial activated carbon (Fujian Yuanli Activated Carbon Co., Ltd., HA, hereinafter the same) and 20g of urea were mechanically stirred until homogeneous. The mixture was placed in a tube furnace and heated to 800℃ (heating rate 10℃ / min) under N2 atmosphere, and stabilized for 6h. The resulting support is denoted as NC-1. 2.57mmol H2PtCl6·6H2O and 0.96mmol BiCl3 were dissolved together in 1.2mol / L hydrochloric acid solution (10ml). 10g of NC-1 was impregnated in the above mixture and dried overnight in an oven at 100℃. The resulting catalyst is denoted as PtBi / NC-1. The mass fraction of Pt is 5.2%, and the mass fraction of Bi is 1.9%.
[0039] The catalyst was placed in a tube furnace and first reduced and activated at 450℃ (heating rate 5℃ / min) under a pure hydrogen atmosphere (flow rate 100 ml / min) at atmospheric pressure for 3 h. Then, the atmosphere was switched to N2, and the mixture was allowed to cool naturally to room temperature. The reduced catalyst was removed, and 0.5 g of the catalyst was transferred to a 50 ml stainless steel autoclave reactor. 10 g of isononol and 20 g of deionized water were added. The gas in the autoclave reactor was replaced five times with 0.3 MPa O2, and then pressurized to 0.3 MPa. The autoclave reactor was heated until it stabilized at 80℃, and then a magnetic stirrer was started (1000 rpm). The reaction was timed. After 24 h, heating and stirring were stopped, and the autoclave reactor was rapidly cooled to room temperature using a cold water bath (0℃). The autoclave reactor was then depressurized (to atmospheric pressure), and the catalyst was separated using a centrifuge. The upper oil phase was collected for chromatographic analysis. The analytical results are shown in Table 1. The products, isonononic acid and isononyl isononanoate, have significantly different boiling points and can be separated using conventional methods in the field. This invention will not elaborate further on the separation of the two products, and the same applies below.
[0040] Example 2
[0041] PtBi / NC-2 catalyst: 10g of commercial activated carbon and 10g of cyanamide were mechanically stirred until homogeneous, placed in a tube furnace, and heated to 700℃ (heating rate 10℃ / min) under N2 atmosphere, and stabilized for 24h. The resulting support is designated NC-2. 3.60mmol H2PtCl6·6H2O and 0.48mmol BiCl3 were dissolved together in 1.2mol / L hydrochloric acid solution (10ml). 10g of NC-2 was impregnated in the above mixture and dried overnight in an oven at 120℃. The resulting catalyst is designated PtBi / NC-2, wherein the mass fraction of Pt is 7.0% and the mass fraction of Bi is 1.0%.
[0042] The catalyst was placed in a tube furnace and first reduced and activated at 550℃ (heating rate 10℃ / min) under a pure hydrogen atmosphere (flow rate 50 ml / min) at atmospheric pressure for 20 h. Then, the atmosphere was switched to N2, and the mixture was allowed to cool naturally to room temperature. The reduced catalyst was removed, and 0.5 g of it was transferred to a 50 ml stainless steel autoclave. 10 g of isononol and 30 g of deionized water were added. The autoclave was purged five times with air at 0.3 MPa, then pressurized to 2 MPa and heated. Once the temperature stabilized at 100℃, a magnetic stirrer was started (1000 rpm), and the reaction time was recorded. After 6 h of reaction, heating and stirring were stopped, and the autoclave was rapidly cooled to room temperature using a cold water bath (0℃). The autoclave was then depressurized (to atmospheric pressure), and the catalyst was separated using a centrifuge. The upper oil phase was collected for chromatographic analysis. The results are shown in Table 1.
[0043] Example 3
[0044] PtBi / NC-3 catalyst: 10g of commercial activated carbon and 10g of dicyandiamide were mechanically stirred until homogeneous. The mixture was placed in a tube furnace and heated to 1000℃ (heating rate 10℃ / min) under N2 atmosphere, and stabilized for 1h. The resulting support is designated NC-3. 3.60mmol H2PtCl6·6H2O and 2.40mmol BiCl3 were dissolved together in 1.2mol / L hydrochloric acid solution (10ml). 10g of NC-3 was impregnated in the above mixture and dried overnight in an oven at 50℃. The resulting catalyst is designated PtBi / NC-3, wherein the mass fraction of Pt is 6.9% and the mass fraction of Bi is 5.0%.
[0045] The catalyst was placed in a tube furnace and first reduced and activated at 300℃ (heating rate 5℃ / min) under a pure hydrogen atmosphere (flow rate 200 ml / min) at atmospheric pressure for 1 h. Then, the atmosphere was switched to N2, and the mixture was allowed to cool naturally to room temperature. The reduced catalyst was removed, and 0.5 g of the catalyst was transferred to a 50 ml stainless steel autoclave reactor. 10 g of isononol was added, and the reactor was purged five times with 0.3 MPa O2. The pressure was then increased to 0.9 MPa, and the reactor was heated until it stabilized at 100℃. A magnetic stirrer was then started (1000 rpm), and the reaction time was recorded. After 72 h of reaction, heating and stirring were stopped, and the reactor was rapidly cooled to room temperature using a cold water bath (0℃). The reactor was then depressurized (to atmospheric pressure), and the catalyst was separated using a centrifuge. The upper oil phase was collected for chromatographic analysis. The results are shown in Table 1.
[0046] Example 4
[0047] PtBi / NC-4 catalyst: 10g of commercial activated carbon and 15g of melamine were mechanically stirred until homogeneous. The mixture was placed in a tube furnace and heated to 800℃ (heating rate 10℃ / min) under N2 atmosphere, and stabilized for 12h. The resulting support is designated NC-4. 0.51mmol H2PtCl6·6H2O and 0.96mmol BiCl3 were dissolved together in 1.2mol / L hydrochloric acid solution (10ml). 10g of NC-4 was impregnated in the above mixture and dried overnight in an oven at 100℃. The resulting catalyst is designated PtBi / NC-4, where the mass fraction of Pt is 1.0% and the mass fraction of Bi is 2.1%.
[0048] The catalyst was placed in a tube furnace and first reduced and activated at 450℃ (heating rate 5℃ / min) under a pure hydrogen atmosphere (flow rate 100 ml / min) at atmospheric pressure for 6 h. Then, the atmosphere was switched to N2, and the mixture was allowed to cool naturally to room temperature. The reduced catalyst was removed, and 0.5 g of the catalyst was transferred to a 50 ml stainless steel autoclave reactor. 2.5 g of isononol and 20 g of deionized water were added. The reactor was purged five times with 0.3 MPa O2, then pressurized to 0.3 MPa and heated. Once the temperature stabilized at 40℃, magnetic stirring (1000 rpm) was started, and the reaction time was recorded. After 24 h of reaction, heating and stirring were stopped, and the reactor was rapidly cooled to room temperature using a cold water bath (0℃). The reactor was then depressurized (to atmospheric pressure), and the catalyst was separated using a centrifuge. The upper oil phase was collected for chromatographic analysis. The analytical results are shown in Table 1.
[0049] Example 5
[0050] PtBi / NC-5 catalyst: 91.6 ml of aniline was dissolved in 800 ml of 1.25 mol / L hydrochloric acid aqueous solution to obtain solution A. 228.8 g of ammonium thiosulfate was dissolved in 400 ml of deionized water to obtain solution B. Solutions A and B were cooled to 4°C. Then, solution B was added to solution A in one go under stirring (1000 rpm), and stirring continued for 24 h. The resulting solid was filtered, washed with deionized water, and dried (overnight in an oven at 120°C) to obtain polyaniline. This polyaniline was then transferred to a tube furnace and carbonized at 1200°C for 6 h under a N2 atmosphere. The resulting support is designated NC-5.
[0051] Dissolve 2.57 mmol H₂PtCl₆·6H₂O and 0.96 mmol BiCl₃ together in 1.2 mol / L hydrochloric acid solution (10 mL). Impregnate 10 g of NC-5 in the above mixture and dry it overnight in an oven at 100 °C. The resulting catalyst is designated PtBi / NC-5, where the mass fraction of Pt is 5.3% and the mass fraction of Bi is 2.2%.
[0052] The catalyst was placed in a tube furnace and first reduced and activated at 450℃ (heating rate 5℃ / min) under a pure hydrogen atmosphere (flow rate 100 ml / min) at atmospheric pressure for 6 h. Then, the atmosphere was switched to N2, and the mixture was allowed to cool naturally to room temperature. The reduced catalyst was removed, and 0.5 g of the catalyst was transferred to a 50 ml stainless steel autoclave reactor. 2.5 g of isononol and 20 g of deionized water were added. The autoclave reactor was purged five times with air at 0.3 MPa, then pressurized to 1 MPa and heated. Once the temperature stabilized at 80℃, a magnetic stirrer was started (1000 rpm), and the reaction time was recorded. After 24 h of reaction, heating and stirring were stopped, and the autoclave reactor was rapidly cooled to room temperature using a cold water bath (0℃). The pressure was then released from the autoclave reactor (to atmospheric pressure), and the catalyst was separated using a centrifuge. The upper oil phase was then collected for chromatographic analysis. The analytical results are shown in Table 1.
[0053] Example 6
[0054] PtBi / NC-6 catalyst: Solution E was prepared by dissolving 1.5 ml of ammonia (30 wt%) and 50 ml of ethanol in 100 ml of deionized water. Solution F was prepared by dissolving 1.0 g of dopamine hydrochloride in 10 ml of deionized water. Solution F was added to solution E in one go while stirring (1000 rpm), and stirring was continued for 30 h. The resulting solid was filtered, washed with deionized water, and dried (overnight in an oven at 120 °C) to obtain polydopamine. This polydopamine was then transferred to a tube furnace and carbonized at 800 °C for 24 h under a N2 atmosphere. The resulting support was designated NC-6.
[0055] Dissolve 2.57 mmol H₂PtCl₆·6H₂O and 0.96 mmol BiCl₃ together in 1.2 mol / L hydrochloric acid solution (10 mL). Impregnate 10 g of NC-6 in the above mixture and dry it overnight in an oven at 100 °C. The resulting catalyst is designated PtBi / NC-6, where the mass fraction of Pt is 5.0% and the mass fraction of Bi is 1.9%.
[0056] The catalyst was placed in a tube furnace and first reduced and activated at 450℃ (heating rate 5℃ / min) under a pure hydrogen atmosphere (flow rate 100 ml / min) at atmospheric pressure for 6 h. Then, the atmosphere was switched to N2, and the mixture was allowed to cool naturally to room temperature. The reduced catalyst was removed, and 0.5 g of the catalyst was transferred to a 50 ml stainless steel autoclave reactor. 10 g of isononol and 10 g of deionized water were added. The reactor was purged five times with 0.3 MPa O2, then pressurized to 0.6 MPa and heated. Once the temperature stabilized at 100℃, a magnetic stirrer was started (1000 rpm), and the reaction time was recorded. After 24 h of reaction, heating and stirring were stopped, and the reactor was rapidly cooled to room temperature using a cold water bath (0℃). The reactor was then depressurized (to atmospheric pressure), and the catalyst was separated using a centrifuge. The upper oil phase was collected for chromatographic analysis. The analytical results are shown in Table 1.
[0057] Example 7
[0058] Cyclic performance of PtBi / NC-1 catalyst: The catalyst after reaction in Example 1 was recovered by centrifugation. The recovered catalyst was washed continuously with water and ethanol, dried (120℃, 12h), and then fed back into the reactor under the reaction conditions in Example 1 for four cycles. The upper oil phase was taken for chromatographic analysis after each cycle. The analytical results are shown in Table 1.
[0059] Comparative Example 1
[0060] PtBi / AC catalyst: Dissolve 2.57 mmol H₂PtCl₆·6H₂O and 0.96 mmol BiCl₃ together in 1.2 mol / L hydrochloric acid solution (10 ml). Impregnate 10 g of commercial activated carbon in the above mixture and dry it overnight in an oven at 100 °C. The resulting catalyst is denoted as PtBi / AC. The mass fraction of Pt is 5.0%, and the mass fraction of Bi is 2.0%.
[0061] The catalyst was placed in a tube furnace and first reduced and activated at 450℃ (heating rate 5℃ / min) under a pure hydrogen atmosphere (flow rate 100 ml / min) at atmospheric pressure for 3 h. Then, the atmosphere was switched to N2, and the mixture was allowed to cool naturally to room temperature. The reduced catalyst was removed, and 0.5 g of the catalyst was transferred to a 50 ml stainless steel autoclave reactor. 10 g of isononol and 20 g of deionized water were added. The gas in the autoclave reactor was replaced five times with 0.3 MPa O2, and then pressurized to 0.3 MPa. The autoclave reactor was heated until it stabilized at 80℃, and then a magnetic stirrer was started (1000 rpm). The reaction was timed. After 24 h, heating and stirring were stopped, and the autoclave reactor was rapidly cooled to room temperature using a cold water bath (0℃). The autoclave reactor was then depressurized (to atmospheric pressure), and the catalyst was separated using a centrifuge. The upper oil phase was collected for chromatographic analysis. The analytical results are shown in Table 1.
[0062] Table 1. Results of catalyst performance in the isononanol oxidation reaction in each example and comparative example.
[0063]
[0064] As can be seen from Examples 1-6, different PtBi / NC catalysts can achieve efficient conversion of isononol to isononanoic acid and isonononoic acid ester in the high-pressure autoclave process (batch reaction process) of isononol oxidation reaction under mild reaction conditions without alkali.
[0065] As can be seen from Example 3, PtBi / NC can achieve efficient conversion of isononyl alcohol to isononanoic acid and isononyl isononanoate without any external solvent.
[0066] As can be seen from Example 7, the PtBi / NC catalyst exhibits excellent stability in the cyclic reuse experiment.
[0067] As can be seen from Comparative Example 1, the reaction activity of PtBi / AC catalyst in the autoclave process and the selectivity of isononanoic acid and isononyl isononanoate are much lower than those of PtBi / NC.
Claims
1. Use of a nitrogen-doped carbon-supported PtBi bimetallic catalyst in the oxidation of isononyl alcohol to prepare isononanoic acid and isononyl isononanoate, characterized in that, The nitrogen-doped carbon-supported PtBi bimetallic catalyst is a catalyst composed of three components: active component Pt, auxiliary agent Bi, and nitrogen-doped carbon support. The nitrogen-doped carbon carrier is obtained by mechanically mixing activated carbon with a nitrogen-containing precursor and then pyrolyzing it at high temperature. The nitrogen-containing precursor includes urea, cyanamide, dicyandiamide, or melamine; or it is obtained by high-temperature pyrolysis of a nitrogen-containing organic polymer, wherein the nitrogen-containing organic polymer includes polyaniline or polydopamine. The catalyst is prepared by the following steps: dissolving Pt precursor and Bi precursor together in hydrochloric acid solution, then loading them onto a nitrogen-doped carbon support by impregnation, and then drying to obtain the catalyst; In application, the catalyst is first placed in a tubular furnace for hydrogen reduction. After cooling to room temperature, the catalyst is loaded into a high-pressure reactor. Then, isononol and deionized water are added to the high-pressure reactor, or isononol is added to the high-pressure reactor alone. The high-pressure reactor is then continuously purged with oxygen-containing gas. The high-pressure reactor is then pressurized to the specified pressure and the temperature is raised. Once the reaction temperature is reached, stirring is started to carry out the reaction.
2. Use according to claim 1, characterized in that, The catalyst has an active component Pt with a mass fraction of 1-7%, an auxiliary agent Bi with a mass fraction of 1-5%, and the remainder is nitrogen-doped carbon support.
3. Use according to claim 1, characterized in that, The activated carbon to nitrogen-containing precursor obtained by mechanically mixing activated carbon and nitrogen-containing precursor and then pyrolyzing at high temperature has a mass ratio of 10:10~20, and the high-temperature pyrolysis conditions are 700~1000℃ for 1~24h under an inert atmosphere; the high-temperature pyrolysis conditions obtained by high-temperature pyrolysis of nitrogen-containing organic polymers are 800~1200℃ for 6~24h under an inert atmosphere.
4. Use according to claim 1, characterized in that, The Pt precursor includes chloroplatinic acid, the Bi precursor includes BiCl3, and the hydrochloric acid solution concentration is 0.5~1.5 mol / L.
5. The use according to claim 1, characterized in that, The drying conditions are 50~120℃ for 6~24 hours.
6. Use according to any one of claims 1 to 5, characterized in that, The reduction conditions are as follows: hydrogen flow rate of 50~200 ml / min, reduction temperature of 300~550℃, heating rate of 5~10℃ / min, reduction time of 1~20 h, and reduction pressure of atmospheric pressure.
7. The use according to any one of claims 1 to 5, characterized in that, The reaction conditions are as follows: the mass ratio of isononol to catalyst is 5~20:1, the mass ratio of deionized water to catalyst is 0~60:1, the oxygen-containing gas includes O2 or air, the O2 pressure is 0.3~0.9MPa, the air pressure is 0.5~2.0MPa, the reaction temperature is 40~100℃, the stirring speed is 600~1000rpm, and the reaction time is 6~72h.
Citation Information
Patent Citations
System and method for preparing isononanoic acid and method for preparing metal organic skeletal catalyst
CN108047027A
Method for preparing isononanoic acid from green oxidation of isononyl alcohol
WO2022116243A1
Copper-based catalyst taking nitrogen-modified activated carbon as carrier as well as preparation method and application thereof
CN111420694A
Solid catalyst for glycerol oxidation and preparation method thereof
CN111545239A