A cobalt-containing monolithic catalyst and mild preparation method and use
By growing cobalt oxide nanoarray structures in situ on a ceramic honeycomb substrate, the problem of uniform and robust loading of cobalt-based catalysts under mild conditions is solved, thereby improving the catalytic performance and applicability of the catalysts and making them suitable for industrial applications.
Patent Information
- Application Number
- CN202410515240.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-26
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-04-26
AI Technical Summary
Existing cobalt-based catalysts are difficult to load uniformly and firmly under mild conditions in the catalytic reaction of toluene combustion, and the preparation conditions are harsh, making them difficult to apply industrially.
After etching the ceramic honeycomb substrate in a strong alkaline solution, cobalt oxide active components are grown in situ on the ceramic honeycomb surface through pre-activation with cobalt nitrate solution, forming a regular nanoarray structure.
This method achieves uniform dispersion and strong bonding of cobalt oxide active components on the ceramic substrate surface, improving the activity and stability of catalytic oxidation degradation of toluene, making it suitable for industrial applications.
Smart Images

Figure CN118356983B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of catalysts, and more particularly to a cobalt-containing monolithic catalyst, a mild preparation method, and its applications. Background Technology
[0002] Volatile organic compounds (VOCs) mainly include alkanes, aromatics, esters, alkenes, carboxylic acids, and alcohols. Existing technologies for VOC removal include catalytic oxidation, adsorption, absorption, biofiltration, membrane filtration, incineration, and combustion. Adsorption technology improves VOC adsorption capacity by enhancing the specific surface area, pore capacity, surface chemical functional groups, and reducing pore size of the adsorbent material, while also allowing for the recovery and reuse of the adsorbent material and VOCs. Biofiltration technology is used to remove VOCs at low to moderate concentrations (<1000 mg / L), but requires regular backwashing of the filter bed. Membrane filtration technology is typically used to separate halogenated VOCs (such as chloroform, trichloroethylene, tetrachloroethylene, etc.) and avoid byproduct formation. Compared to the above technologies, catalytic oxidation is considered a highly efficient and economical advanced oxidation technology for VOC removal. Toxic VOCs can be oxidized into CO2, water, and other less harmful substances at relatively low temperatures. Lower temperatures mean relatively lower fuel costs and less formation of dioxins and toxic products. Catalytic oxidation is suitable for the continuous treatment of low-concentration VOCs. However, existing VOCs decomposition catalysts are mainly divided into noble metal catalysts and catalysts containing transition metal oxides. Noble metal catalysts are limited in large-scale industrial application due to their high cost; while the selection of transition metal oxides is crucial for catalysts containing transition metal oxides. In the toluene combustion catalytic reaction, no reports have yet described the development of a uniformly supported, robust, and high-performance cobalt-based catalyst under mild conditions using a self-growth method.
[0003] Currently, cobalt-based catalysts are mainly classified into two macroscopic forms: particulate and monolithic catalysts. Particulate catalysts have high bed pressure drop, making them unsuitable for treating high-space-velocity toluene gas. Monolithic catalysts often use activated carbon honeycomb, metal, or ceramic honeycomb as the structured substrate. For example, Chinese patent CN109261164A first prepares catalyst powder, then formulates a catalyst slurry, and finally loads it onto a honeycomb support through an immersion coating process to form a monolithic catalyst. This effectively reduces bed pressure drop during use and achieves effective removal of the target gas under low temperature, high space velocity, and high humidity conditions. However, this method only provides a simple coating loading method between the catalyst and the support and is difficult to implement on a smooth metal substrate. Chinese patent CN113477246A produces a monolithic catalyst by direct in-situ growth on a honeycomb support via a hydrothermal reaction. Compared to the immersion-coating process, this method successfully grows a manganese oxide coating in situ on a metal substrate, with a tighter bond at the loading interface, which helps improve catalytic performance. However, it is not prepared under mild conditions and has high requirements for preparation conditions, making it difficult to apply in industrial applications. Summary of the Invention
[0004] The purpose of this invention is to propose a mild preparation method for a cobalt-containing monolithic catalyst. This method involves directly placing a ceramic honeycomb in a cobalt-containing precursor liquid, which allows cobalt oxide active components to grow in situ on the surface of the ceramic honeycomb. The newly formed cobalt oxide active component particles can not only be uniformly dispersed on the surface of the ceramic substrate, but also firmly bonded to the surface of the ceramic substrate.
[0005] The present invention also proposes a cobalt-containing monolithic catalyst, which is prepared by the above-described mild preparation method.
[0006] The present invention also proposes a toluene catalyst comprising the aforementioned cobalt-containing monolithic catalyst.
[0007] The present invention also proposes a method for the catalytic decomposition of toluene, which uses the aforementioned cobalt-containing monolithic catalyst.
[0008] The present invention also proposes the use of a catalyst in the catalytic decomposition of toluene.
[0009] To achieve this objective, the present invention adopts the following technical solution: A mild method for preparing a cobalt-containing monolithic catalyst includes the following steps: (1) Pretreatment: The ceramic honeycomb substrate is immersed in a strong alkaline solution for etching, then taken out, rinsed with water, and calcined at 400-600℃; (2) Pre-activation: After immersing the ceramic honeycomb substrate from step (1) in a 0.01-0.04 mol / L cobalt nitrate solution at room temperature, hydroxycobalt nitrate seed crystals are formed on the ceramic honeycomb substrate, and then the substrate is removed and dried. (3) Preparation of cobalt precursor solution: Cobalt nitrate hexahydrate, urea and deionized water are mixed and stirred to obtain cobalt precursor solution. The solid amounts of cobalt nitrate and urea are slowly added in a molar ratio of 1:(0.5-2). (4) The pre-activated sample from step (2) is suspended in the cobalt precursor liquid obtained in step (3) and reacted under water bath heating and continuous stirring conditions; it is then removed, rinsed and dried, and calcined at 200-500℃ to obtain a cobalt-containing monolithic catalyst.
[0010] The following steps can be optimized: (1) Pretreatment: Immerse the ceramic honeycomb substrate in a 0.05-0.2 mol / L strong alkaline solution for etching, maintain 60-100℃, then take it out, rinse it with water, and calcine it at 400-600℃; (2) Pre-activation: After immersing the ceramic honeycomb substrate from step (1) in a 0.01-0.04 mol / L cobalt nitrate solution at room temperature, hydroxycobalt nitrate seed crystals are formed on the ceramic honeycomb substrate, and then the substrate is removed and dried. (3) Preparation of cobalt precursor solution: Mix cobalt nitrate hexahydrate, urea and deionized water, stir to obtain cobalt precursor solution; adjust the concentration of cobalt nitrate to 0.2-0.8 mol / L and the amount of urea added to 0.2-0.8 mol / L; In step (4), the mass percentage of cobalt in the cobalt-containing monolithic catalyst is 10-30 wt%.
[0011] Alternatively, in step (1), the strong alkaline solution can be a sodium hydroxide solution or a potassium hydroxide solution.
[0012] Alternatively, in step (1), a silicon carbide honeycomb substrate, a molecular sieve honeycomb substrate, or an alumina honeycomb substrate may be used instead of a ceramic honeycomb substrate.
[0013] A cobalt-containing monolithic catalyst is prepared by the mild preparation method described above for a cobalt-containing monolithic catalyst.
[0014] A toluene catalyst includes: the aforementioned cobalt-containing monolithic catalyst.
[0015] A method for catalytic decomposition of toluene uses a cobalt-containing monolithic catalyst as described above. The cobalt-containing monolithic catalyst is placed in the reaction tube of a gas-solid phase reaction device, and then toluene gas is introduced into the reaction tube.
[0016] The use of a catalyst in the catalytic decomposition of toluene, said catalyst being prepared by the mild preparation method of the aforementioned cobalt-containing monolithic catalyst.
[0017] Compared with the prior art, one of the above technical solutions has the following beneficial effects: This solution provides a mild preparation method for a cobalt-containing monolithic catalyst. This method does not require the pre-preparation of cobalt-containing active component powder. Instead, the ceramic honeycomb is directly placed in a cobalt-containing precursor liquid, and cobalt oxide active components are grown in situ on the surface of the ceramic honeycomb. The newly formed cobalt oxide active component particles can not only be uniformly dispersed on the surface of the ceramic substrate, but also firmly bonded to the surface of the ceramic substrate. This solves the problem that monolithic catalysts, where the catalyst and support are only coated and thus difficult to achieve on a smooth metal substrate, and the problem that the preparation conditions of monolithic catalysts are harsh and difficult to use in industrial applications. Attached Figure Description
[0018] Figure 1 This is a sample image of the monolithic ceramic honeycomb catalyst of cobalt oxide from Example A; Figure 2 This is an electron microscope image of the monolithic ceramic honeycomb catalyst of cobalt oxide in Example A. Detailed Implementation
[0019] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the specification of this invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0020] A mild method for preparing a cobalt-containing monolithic catalyst, characterized by comprising the following steps: (1) Pretreatment: The ceramic honeycomb substrate is immersed in a strong alkaline solution for etching, then taken out, rinsed with water, and calcined at 400-600℃; This technical solution uses strong alkali to perform alkaline etching on the ceramic honeycomb substrate. On the one hand, the strong alkali etching creates a porous structure on the surface of the ceramic honeycomb substrate, increasing the specific surface area of the blank substrate itself, which is more conducive to the uniform deposition of cobalt hydroxynitrate in the subsequent step. On the other hand, the alkaline etching treatment can make the substrate surface weakly alkaline, which can be pre-activated with cobalt nitrate solution in step (2) to form cobalt hydroxynitrate seed crystals on the substrate surface, thereby inducing the deposition process in the subsequent step (4) to be more targeted and more conducive to the formation of cobalt oxide array structure.
[0021] The choice of honeycomb substrate ensures the stability of the honeycomb structure during alkaline etching; and ceramic substrates, due to their excellent chemical stability, can better form surface defect structures and residual weak alkalinity during alkaline etching pretreatment, which is more conducive to the subsequent formation of a regular cobalt oxide array structure.
[0022] (2) Pre-activation: After immersing the ceramic honeycomb substrate from step (1) in a 0.01-0.04 mol / L cobalt nitrate solution at room temperature, hydroxycobalt nitrate seed crystals are formed on the ceramic honeycomb substrate, and then the substrate is removed and dried. After alkaline etching pretreatment of the ceramic honeycomb substrate, a weakly alkaline environment is created on the surface. Then, pre-activation is achieved by immersion in a cobalt nitrate solution, allowing hydroxyl cobalt nitrate nuclei to form in situ on the substrate surface. Utilizing the inductive effect of these nuclei, in step (4), cobalt ions in the cobalt precursor solution undergo a slow chemical reaction with hydroxide ions obtained from the thermal decomposition of urea, generating hydroxyl cobalt nitrate crystals. These crystals continuously deposit and grow around the nuclei, ultimately forming a regular cobalt oxide nanoarray structure on the substrate surface. Furthermore, because the cobalt oxide nanoarray structure is formed on the honeycomb substrate surface using an in-situ growth method, compared to the cobalt-containing monolithic catalyst prepared by the immersion-coating process, the cobalt oxide active component particles in the monolithic catalyst formed by this method are more firmly loaded on the substrate surface and more uniformly distributed.
[0023] (3) Preparation of cobalt precursor solution: Cobalt nitrate hexahydrate, urea and deionized water are mixed and stirred to obtain cobalt precursor solution. The solid amounts of cobalt nitrate and urea are slowly added in a molar ratio of 1:(0.5-2). This technical solution uses cobalt nitrate as a cobalt precursor because it is easier to slowly generate cobalt hydroxynitrate crystals under the induction of crystal nuclei by controlling an alkaline environment, thereby forming a cobalt oxide array structure on the substrate surface. The generation of cobalt hydroxynitrate crystals is more controllable. At the same time, choosing cobalt nitrate also makes it easier to form cobalt hydroxynitrate crystal nuclei in the pre-activation step by utilizing the weak alkalinity of the substrate surface.
[0024] The ratio of cobalt nitrate to solid urea can be adjusted to 1:(0.5-2). This ratio affects the generation and deposition rate of cobalt hydroxynitrate in step (4), and thus affects the size of the cobalt oxide nanoparticles and the density of the array structure formed in the resulting catalyst. A ratio of approximately 1:1 is optimal.
[0025] The cobalt precursor liquid can be in the process of being prepared or in the state after being prepared. This scheme can be selected as needed to control the reaction process between the pre-activated sample and the cobalt precursor liquid in step (4). (4) The pre-activated sample from step (2) is suspended in the cobalt precursor liquid obtained in step (3) and reacted under water bath heating and continuous stirring conditions; it is then removed, rinsed and dried, and calcined at 200-500℃ to obtain a cobalt-containing monolithic catalyst.
[0026] The cobalt oxide nanoarray structure formed on the surface of the monolithic cobalt oxide catalyst after step (4) is more conducive to the uniform dispersion of the cobalt oxide active component on the substrate surface, and can expose more active sites to contact the reactant toluene, thereby increasing the reaction rate. On the other hand, the regular nanoarray structure can make the cobalt oxide active component have more oxygen vacancies, enhance its oxidation / reduction cycle efficiency and stability, thereby improving the activity of catalytic oxidation and degradation of toluene.
[0027] This solution provides a mild preparation method for a cobalt-containing monolithic catalyst. This method does not require the pre-preparation of cobalt-containing active component powder. Instead, the ceramic honeycomb is directly placed in a cobalt-containing precursor liquid, and cobalt oxide active components are grown in situ on the surface of the ceramic honeycomb. The newly formed cobalt oxide active component particles can not only be uniformly dispersed on the surface of the ceramic substrate, but also firmly bonded to the surface of the ceramic substrate. This solves the problem that monolithic catalysts, where the catalyst and support are only coated and thus difficult to achieve on a smooth metal substrate, and the problem that the preparation conditions of monolithic catalysts are harsh and difficult to use in industrial applications.
[0028] Steps (1) - pretreatment, (2) - preactivation, (3) - preparation of cobalt precursor liquid and step (4) of this scheme are all carried out under mild conditions. Mild conditions refer to reaction environments with low preparation requirements. Non-heating requirements can be defined as being carried out at room temperature and normal pressure. Heating requirements can be defined as being above room temperature and below 100°C, at normal pressure. For example, water bath heating is a mild condition, and its maximum temperature is 100°C. In some embodiments, oil baths can be used instead of water baths at temperatures below 200°C, for example, at normal pressure.
[0029] In the preferred embodiment, the following operational steps are included: (1) Pretreatment: Immerse the ceramic honeycomb substrate in a 0.05-0.2 mol / L strong alkaline solution for etching, maintain 60-100℃, then take it out, rinse it with water, and calcine it at 400-600℃; (2) Pre-activation: After immersing the ceramic honeycomb substrate from step (1) in a 0.01-0.04 mol / L cobalt nitrate solution at room temperature, hydroxycobalt nitrate seed crystals are formed on the ceramic honeycomb substrate, and then the substrate is removed and dried. (3) Preparation of cobalt precursor solution: Mix cobalt nitrate hexahydrate, urea and deionized water, stir to obtain cobalt precursor solution; adjust the concentration of cobalt nitrate to 0.2-0.8 mol / L and the amount of urea added to 0.2-0.8 mol / L; In step (4), the mass percentage of cobalt in the cobalt-containing monolithic catalyst is 10-30 wt%.
[0030] As the optimal embodiment, this scheme uses a 0.05-0.2 mol / L strong alkaline solution for etching in the pretreatment, and a 0.01-0.04 mol / L cobalt nitrate solution as the impregnation liquid. The amount of cobalt nitrate and urea added is also adjusted to 0.2-0.8 mol / L. Finally, it can ensure that a cobalt-containing monolithic catalyst with a mass percentage of 10-30 wt% is stably obtained in step (4). Therefore, this invention can achieve self-growth and stably obtain a cobalt-containing monolithic catalyst with a mass percentage of 10-30 wt% under mild conditions (normal pressure, low temperature), which has good prospects for industrial application.
[0031] Alternatively, in step (1), the strong alkaline solution can be a sodium hydroxide solution or a potassium hydroxide solution.
[0032] Alternatively, in step (1), a silicon carbide honeycomb substrate, a molecular sieve honeycomb substrate, or an alumina honeycomb substrate may be used instead of a ceramic honeycomb substrate.
[0033] This solution can also use silicon carbide honeycomb substrates, molecular sieve honeycomb substrates, or alumina honeycomb substrates instead of ceramic honeycomb substrates. During the alkaline etching pretreatment process, surface defect structures and residual weak alkalinity can also be formed on silicon carbide honeycomb substrates, molecular sieve honeycomb substrates, or alumina honeycomb substrates, so as to form a more regular cobalt oxide array structure in the subsequent process.
[0034] A cobalt-containing monolithic catalyst is prepared by the mild preparation method described above for a cobalt-containing monolithic catalyst.
[0035] A toluene catalyst comprising the aforementioned cobalt-containing monolithic catalyst.
[0036] A method for catalytic decomposition of toluene uses a cobalt-containing monolithic catalyst as described above. The cobalt-containing monolithic catalyst is placed in the reaction tube of a gas-solid phase reaction device, and then toluene gas is introduced into the reaction tube.
[0037] The cobalt oxide nanoarray structure formed on the surface of the monolithic cobalt oxide catalyst is beneficial in two ways. First, it facilitates the uniform dispersion of the cobalt oxide active component on the substrate surface, exposing more active sites for contact with the reactant toluene and increasing the reaction rate. Second, the cobalt-containing monolithic catalyst in this scheme is pretreated, which creates defect structures on the ceramic honeycomb surface, enabling more uniform distribution of Co3O4 and enhancing the Co3O4 / CHC reduction / oxidation cycle, thereby enhancing the catalytic oxidation activity of toluene.
[0038] The use of a catalyst in the catalytic decomposition of toluene, said catalyst being prepared by the mild preparation method of the aforementioned cobalt-containing monolithic catalyst.
[0039] The following are performance tests performed in the examples below: 1. Electron microscope image analysis: The catalyst sample was first subjected to gold spraying treatment to increase conductivity, and then placed in the high-vacuum sample chamber of a Hitachi S-3400N II scanning electron microscope for microscopic morphology observation, so as to obtain electron microscope images at different magnifications.
[0040] 2. Content analysis: An X-ray energy spectrometer supporting the S-3400N II scanning electron microscope was used to further analyze the element types and contents of the micro-area components of the catalyst sample.
[0041] 3. Toluene purification performance: The catalyst sample was placed in the reaction tube of the gas-solid phase catalytic activity evaluation device, and the catalytic oxidation purification of toluene was used as the probe reaction. Under the conditions of inlet toluene concentration of 1.0 g / m 3 and volumetric space velocity of 10000 h -1 , the catalyst activity test was carried out, and the toluene concentration at the outlet was detected by a gas chromatograph. Specifically, the toluene catalytic oxidation purification reaction was carried out on a fixed-bed flow reaction device. A monolithic catalyst of a certain size was loaded into a reaction tube (diameter ≈ 9 mm). Toluene was brought into the reaction tube in the form of vapor by air with a certain flow rate for reaction. The toluene injection concentration (Co = 1.0 g / m 3 ), space velocity GHSV (=10000 h -1 ) and reaction temperature were adjusted. The outlet effluent was monitored online by an HP6820 gas chromatography FID detector, and the experimental data were collected after the reaction was stabilized for 3 h. The reaction temperatures corresponding to 10% and 90% toluene conversion were recorded as the light-off temperature T 10 and the complete conversion temperature T 90 , respectively.
[0042] Example A: (1) Surface pretreatment of ceramic honeycomb substrate: The ceramic honeycomb substrate was immersed in a 0.10 mol / L sodium hydroxide solution, kept at 90°C for 1 h, then taken out, washed with water, and calcined at 500°C for 1 h; (2) Pre-activation of substrate surface: The ceramic honeycomb substrate pretreated in step (1) was immersed in a 0.02 mol / L cobalt nitrate solution at room temperature for 30 min, then taken out and dried at 120°C for 2 h; (3) Preparation of cobalt precursor solution: Cobalt nitrate hexahydrate, urea and deionized water were mixed and continuously stirred at 1000 r / min for 0.5 h to obtain a cobalt precursor solution; Wherein, the concentration of cobalt nitrate was 0.6 mol / L, and the addition amount of urea was 0.6 mol / L. The solid amounts of cobalt nitrate and urea were continuously added at a molar ratio of 1:1 for preparation until step (4) was completed; (4) The pre-activated sample from step (2) was suspended in the cobalt precursor liquid obtained in step (3) and reacted for 12 hours in a 90°C water bath with continuous stirring at 1500 r / min. Then, it was removed, rinsed with water, dried at 80°C for 4 hours, and calcined at 300°C for 4 hours to obtain a monolithic cobalt oxide honeycomb catalyst, such as... Figure 1 .
[0043] The monolithic honeycomb catalyst of cobalt oxide in Example A was analyzed by electron microscopy and its content was determined. The electron microscopy analysis is as follows: Figure 2 As shown in the figure; the content analysis is shown in Table 1.
[0044]
[0045] illustrate: 1. For example Figure 2 As shown, the newly generated cobalt oxide active components are mainly arranged in a regular manner in the form of nanowires on the surface of the ceramic substrate, forming a cobalt oxide array structure. This array structure can effectively avoid the overlap and aggregation of the cobalt oxide catalytic active components and form a rich porous structure, which is more conducive to its full contact with the reactants in subsequent catalytic reactions, thereby improving the catalytic oxidation performance.
[0046] 2. As shown in Table 1, in the sample composition detected by X-ray energy dispersive spectroscopy (EDS), Al, Si, and Mg elements belong to the ceramic substrate, while Co and a large amount of O elements can be attributed to cobalt oxides loaded on the surface of the ceramic substrate. Furthermore, the content of Al, Si, and Mg elements belonging to the ceramic substrate is much lower than the content of Co and O elements belonging to the cobalt oxides, further indicating that the newly formed cobalt oxide active components are uniformly deposited and cover the surface of the ceramic honeycomb substrate. Simultaneously, since the EDS can only detect elemental composition at a depth of approximately 1 micrometer on the sample surface, this further indicates that the thickness of the cobalt oxide array catalytic active layer formed on the surface of the ceramic honeycomb substrate is very thin (less than 1 micrometer). This not only facilitates the firm loading of the catalytic layer on the substrate surface but also better avoids the overlapping and aggregation of cobalt oxide active components within the catalytic layer.
[0047] Secondly, this method can obtain a cobalt-containing monolithic catalyst with a cobalt content of 11.75% by mass, combined with... Figure 2It is evident that the cobalt-containing active component can be firmly loaded and uniformly dispersed on the surface of the ceramic honeycomb substrate. Furthermore, the preparation conditions in Example A are mild, have no requirements on the ceramic shape, and exhibit strong applicability and promising industrialization prospects. In other words, this preparation method does not require pre-preparation of cobalt-containing active component powder; it only requires directly placing the ceramic honeycomb in a cobalt-containing precursor liquid to allow for in-situ growth of the cobalt oxide active component on the ceramic honeycomb surface. The newly formed cobalt oxide active component particles not only disperse uniformly on the ceramic substrate surface but also firmly bind to it. This solves the problem of monolithic catalysts where the catalyst and support are only loaded through a coating, making it difficult to achieve on smooth metal substrates, and the problem of the harsh preparation conditions of monolithic catalysts hindering industrial application.
[0048] Comparative Example A1: (1) Pre-activation of substrate surface: The ceramic honeycomb substrate was immersed in 0.02 mol / L cobalt nitrate solution at room temperature for 30 min, and then dried at 120℃ for 2 h; (2) Preparation of cobalt precursor solution: Cobalt nitrate hexahydrate, urea and deionized water were mixed and stirred continuously at 1000 r / min for 0.5 h to obtain cobalt precursor solution; The concentration of cobalt nitrate is 0.6 mol / L, and the amount of urea added is 0.6 mol / L. The cobalt nitrate and urea solids are continuously added in a molar ratio of 1:1 until step (3) is completed. (3) The pre-activated sample from step (1) is suspended in the cobalt precursor liquid obtained in step (2) and reacted for 12 hours in a 90°C water bath with continuous stirring at 1500 r / min. Then it is taken out, rinsed with water, dried at 80°C for 4 hours, and calcined at 300°C for 4 hours to obtain a cobalt oxide monolithic honeycomb catalyst.
[0049] Comparative Example A2: (1) Surface pretreatment of ceramic honeycomb substrate: The ceramic honeycomb substrate is immersed in 0.10 mol / L sodium hydroxide solution and kept at 90℃ for 1 h. Then it is taken out, rinsed with water, and calcined at 500℃ for 1 h. (2) Preparation of cobalt precursor solution: Cobalt nitrate hexahydrate, urea and deionized water were mixed and stirred continuously at 1000 r / min for 0.5 h to obtain cobalt precursor solution; The concentration of cobalt nitrate is 0.6 mol / L, and the amount of urea added is 0.6 mol / L. The cobalt nitrate and urea solids are continuously added in a molar ratio of 1:1 until step (3) is completed. (3) The sample from step (1) was suspended in the cobalt precursor liquid obtained in step (2) and reacted for 12 hours in a water bath at 90°C and under continuous stirring at 1500 r / min. Then it was taken out, rinsed with water, dried at 80°C for 4 hours, and calcined at 300°C for 4 hours to obtain a monolithic cobalt oxide honeycomb catalyst.
[0050] The toluene purification performance of Example A and Comparative Examples A1 and A2 was tested, and the results are shown in Table 2.
[0051]
[0052] illustrate: 1. As can be seen from the comparison between Example A and Comparative Example A1, Comparative Example A1 did not perform surface pretreatment of the ceramic honeycomb substrate, but directly performed surface preactivation of the substrate. The Ta of Comparative Example A1... 10 At 240℃, T 90 The temperature is 270℃. This method pre-treats the ceramic honeycomb substrate by, on the one hand, creating a porous structure on the surface of the ceramic honeycomb substrate through strong alkaline etching, increasing the specific surface area of the blank substrate itself, which is more conducive to the uniform deposition of cobalt hydroxynitrate in the subsequent process; on the other hand, the alkaline etching treatment can make the substrate surface weakly alkaline, which can be pre-activated with cobalt nitrate solution in the substrate surface pre-activation step to form cobalt hydroxynitrate seed crystals on the substrate surface, providing targeting in the induction of subsequent deposition processes, and is more conducive to the formation of cobalt oxide array structures; Example A's T 10 The temperature is 190℃, T 90 The temperature was 220°C. As a result, the deposition of cobalt hydroxynitrate in Comparative Example A1 decreased uniformly and was not conducive to the formation of an array structure of cobalt oxide, which led to a lower toluene conversion rate in Comparative Example A1 than in Example A.
[0053] 2. Comparison between Example A and Comparative Example A2 shows that Comparative Example A2 did not perform pre-activation of the ceramic honeycomb substrate, but directly reacted the pretreated ceramic honeycomb substrate with the cobalt precursor liquid; the T of Comparative Example A2... 10 At 250℃, T 90 The temperature is 280℃; pre-activation is based on creating a weakly alkaline environment on the surface of the pretreated ceramic honeycomb substrate. During impregnation with cobalt nitrate solution, hydroxyl cobalt nitrate nuclei can be formed in situ on the substrate surface. Then, utilizing the inductive effect of the nuclei, cobalt ions in the cobalt precursor solution undergo a slow chemical reaction with hydroxide ions obtained from the thermal decomposition of urea, generating hydroxyl aluminum nitrate crystals. These crystals continuously deposit and grow around the nuclei, ultimately forming a regular cobalt oxide nanoarray structure on the substrate surface. Therefore, the T in Example A... 10 The temperature is 190℃, T 90The temperature was 220°C. As a result, since Comparative Example A2 was not pre-activated, it was not conducive to the formation of aluminum hydroxynitrate crystals, which was not conducive to obtaining a regular cobalt oxide nanoarray structure. Therefore, the toluene conversion rate of Comparative Example A2 was lower than that of Example A.
[0054] In summary, the monolithic cobalt oxide honeycomb catalyst prepared by this method through pretreatment steps of the ceramic honeycomb substrate, preactivation steps of the ceramic honeycomb substrate, preparation steps of the cobalt precursor liquid, and mild reaction steps, has a cobalt oxide nanoarray structure formed on its surface. On the one hand, it is more conducive to the uniform dispersion of the cobalt oxide active component on the substrate surface, and can expose more active sites to contact the reactant toluene, thereby improving the reaction rate. On the other hand, the regular nanoarray structure can make the cobalt oxide active component have more oxygen vacancies, enhancing its efficiency and stability of oxidation / reduction cycle, thereby improving the activity of catalytic oxidation and degradation of toluene.
[0055] Example B: (1) Surface pretreatment of ceramic honeycomb substrate: The ceramic honeycomb substrate was immersed in 0.05 mol / L potassium hydroxide solution and kept at 70℃ for 4 h. Then it was taken out, rinsed with water, and calcined at 400℃ for 5 h. (2) Pre-activation of substrate surface: The ceramic honeycomb substrate pretreated in step (1) was immersed in 0.01 mol / L cobalt nitrate solution at room temperature for 20 min, and then dried at 110℃ for 5 h. (3) Preparation of cobalt precursor solution: Cobalt nitrate hexahydrate, urea and deionized water are mixed and stirred continuously at 700 r / min for 1 h to obtain cobalt precursor solution; The concentration of cobalt nitrate is 0.8 mol / L, and the amount of urea added is 0.8 mol / L; the cobalt nitrate and urea solids are added and prepared in a molar ratio of 1:2, which is completed before step (4); (4) The pre-activated sample from step (2) is suspended in the cobalt precursor liquid obtained in step (3) and reacted for 30 h in an 80°C water bath with continuous stirring at 1600 r / min. Then it is taken out, rinsed with water, dried at 75°C for 5 h, and calcined at 500°C for 4 h to obtain a cobalt oxide monolithic honeycomb catalyst.
[0056] Example C: (1) Surface pretreatment of ceramic honeycomb substrate: The ceramic honeycomb substrate was immersed in 0.2 mol / L sodium hydroxide solution and kept at 90℃ for 5 h. Then it was taken out, rinsed with water, and calcined at 550℃ for 3 h. (2) Pre-activation of substrate surface: The ceramic honeycomb substrate after step (1) pretreatment is immersed in 0.04 mol / L cobalt nitrate solution at room temperature for 75 min, and then taken out and dried at 115℃ for 2 h; (3) Preparation of cobalt precursor solution: Cobalt nitrate hexahydrate, urea and deionized water were mixed and stirred continuously at 1300 r / min for 0.5 h to obtain cobalt precursor solution; The concentration of cobalt nitrate is 0.5 mol / L, and the amount of urea added is 0.5 mol / L; the cobalt nitrate and urea solids are added and prepared in a molar ratio of 1:0.5, which is completed before step (4); (4) The pre-activated sample from step (2) is suspended in the cobalt precursor liquid obtained in step (3) and reacted for 7 hours in a water bath at 990°C and under continuous stirring at 1300 r / min. Then it is taken out, rinsed with water, dried at 110°C for 4 hours, and calcined at 200°C for 5 hours to obtain a cobalt oxide monolithic honeycomb catalyst.
[0057] Example D: (1) Surface pretreatment of silicon carbide honeycomb substrate: The silicon carbide honeycomb substrate was immersed in 0.1 mol / L sodium hydroxide solution and kept at 85℃ for 10 h. Then it was taken out, rinsed with water, and calcined at 600℃ for 2 h. (2) Pre-activation of substrate surface: The silicon carbide honeycomb substrate pretreated in step (1) was immersed in 0.03 mol / L cobalt nitrate solution at room temperature for 45 min, and then dried at 110℃ for 2 h. (3) Preparation of cobalt precursor solution: Cobalt nitrate hexahydrate, urea and deionized water are mixed and stirred continuously at 1400 r / min for 1 h to obtain cobalt precursor solution; The concentration of cobalt nitrate is 0.3 mol / L, and the amount of urea added is 0.3 mol / L; the cobalt nitrate and urea solids are added and prepared in a molar ratio of 1:1.1, which is completed before step (4); (4) The pre-activated sample from step (2) is suspended in the cobalt precursor liquid obtained in step (3) and reacted for 9 hours in a 90°C water bath with continuous stirring at 1300 r / min. Then it is taken out, rinsed with water, dried at 120°C for 4 hours, and calcined at 400°C for 4 hours to obtain a cobalt oxide monolithic honeycomb catalyst.
[0058] Example E: (1) Surface pretreatment of molecular sieve honeycomb substrate: The molecular sieve honeycomb substrate was immersed in 0.15 mol / L potassium hydroxide solution and kept at 90℃ for 3 h. Then it was taken out, rinsed with water, and calcined at 450℃ for 3 h. (2) Pre-activation of substrate surface: The molecular sieve honeycomb substrate pretreated in step (1) was immersed in 0.02 mol / L cobalt nitrate solution at room temperature for 30 min, and then dried at 120℃ for 1 h. (3) Preparation of cobalt precursor solution: Cobalt nitrate hexahydrate, urea and deionized water were mixed and stirred continuously at 1500 r / min for 0.5 h to obtain cobalt precursor solution; The concentration of cobalt nitrate is 0.7 mol / L, and the amount of urea added is 0.7 mol / L; the cobalt nitrate and urea solids are added and prepared in a molar ratio of 1:1, which is completed before step (4); (4) The pre-activated sample from step (2) is suspended in the cobalt precursor liquid obtained in step (3) and reacted for 10 h in a water bath at 60 °C and under continuous stirring at 1600 r / min. Then it is taken out, rinsed with water, dried at 120 °C for 4 h, and calcined at 350 °C for 4 h to obtain a cobalt oxide monolithic honeycomb catalyst.
[0059] Example F: (1) Surface pretreatment of alumina honeycomb substrate: The alumina honeycomb substrate was immersed in 0.2 mol / L sodium hydroxide solution and kept at 85℃ for 2 h. Then it was taken out, rinsed with water, and calcined at 500℃ for 2 h. (2) Pre-activation of substrate surface: The alumina honeycomb substrate pretreated in step (1) was immersed in 0.02 mol / L cobalt nitrate solution at room temperature for 40 min, and then dried at 120℃ for 1 h. (3) Preparation of cobalt precursor solution: Cobalt nitrate hexahydrate, urea and deionized water were mixed and stirred continuously at 1500 r / min for 0.5 h to obtain cobalt precursor solution; The concentration of cobalt nitrate is 0.55 mol / L, and the amount of urea added is 0.55 mol / L; the cobalt nitrate and urea solids are added and prepared in a molar ratio of 1:1, which is completed before step (4); (4) The pre-activated sample from step (2) is suspended in the cobalt precursor liquid obtained in step (3) and reacted for 8 hours in a 100°C water bath with continuous stirring at 1200 r / min. Then it is taken out, rinsed with water, dried at 110°C for 4 hours, and calcined at 300°C for 5 hours to obtain a cobalt oxide monolithic honeycomb catalyst.
[0060] The content of BF in the example was analyzed and its toluene purification performance was tested. The results are shown in Table 3.
[0061]
[0062] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.
Claims
1. A mild method for preparing a monolithic cobalt-containing catalyst for catalyzing toluene, characterized in that, The following steps are included: (1) Pretreatment: The ceramic honeycomb substrate is immersed in a strong alkaline solution for etching, then taken out, rinsed with water, and calcined at 400-600℃; (2) Pre-activation: After immersing the ceramic honeycomb substrate from step (1) in a 0.01-0.04 mol / L cobalt nitrate solution at room temperature, hydroxycobalt nitrate seed crystals are formed on the ceramic honeycomb substrate, and then the substrate is removed and dried. (3) Preparation of cobalt precursor solution: Cobalt nitrate hexahydrate, urea and deionized water are mixed and stirred to obtain cobalt precursor solution. The solid amounts of cobalt nitrate and urea are slowly added in a molar ratio of 1:(0.5-2). (4) The pre-activated sample from step (2) is suspended in the cobalt precursor liquid obtained in step (3) and reacted under water bath heating and continuous stirring conditions; it is then removed, rinsed and dried, and calcined at 200-500℃ to obtain a cobalt-containing monolithic catalyst.
2. The mild preparation method of the monolithic cobalt-containing catalyst for catalyzing toluene according to claim 1, characterized in that, The following steps are included: (1) Pretreatment: Immerse the ceramic honeycomb substrate in a 0.05-0.2 mol / L strong alkaline solution for etching, maintain 60-100℃, then take it out, rinse it with water, and calcine it at 400-600℃; (2) Pre-activation: After immersing the ceramic honeycomb substrate from step (1) in a 0.01-0.04 mol / L cobalt nitrate solution at room temperature, hydroxycobalt nitrate seed crystals are formed on the ceramic honeycomb substrate, and then the substrate is removed and dried. (3) Preparation of cobalt precursor solution: Mix cobalt nitrate hexahydrate, urea and deionized water, stir to obtain cobalt precursor solution; adjust the concentration of cobalt nitrate to 0.2-0.8 mol / L and the concentration of urea to 0.2-0.8 mol / L; In step (4), the mass percentage of cobalt in the cobalt-containing monolithic catalyst is 10-30 wt%.
3. A mild preparation method for a cobalt-containing monolithic catalyst for catalyzing toluene according to claim 1, characterized in that, In step (1), the strong alkaline solution is a sodium hydroxide solution or a potassium hydroxide solution.
4. A mild preparation method for a cobalt-containing monolithic catalyst for catalyzing toluene according to claim 1, characterized in that, In step (1), a molecular sieve honeycomb substrate is used instead of a ceramic honeycomb substrate.
5. A cobalt-containing monolithic catalyst, characterized in that, It is prepared by a mild preparation method of a cobalt-containing monolithic catalyst for catalytic toluene as described in any one of claims 1-4.
Citation Information
Patent Citations
Preparation of copper and cobalt codoped manganese-based catalyst and application of catalyst to low-concentration ozonolysis
CN109261164A
Manganese-containing integral electric auxiliary metal honeycomb catalyst, preparation method and application thereof
CN113477246A
Metal oxide nanorod arrays on monolithic substrates
CN104080728A
Metal substrate supported catalyst in alkaline system and preparation method and application thereof
CN112958111A