A system and method for mitigating local undercooling of an inner arc surface of a wide slab

By replacing the inner arc support rollers in the secondary cooling zone of the slab continuous casting machine with straight rollers and setting air jet holes, high-pressure gas is used to spray secondary cooling water, which solves the problem of local overcooling on the inner arc surface of the thick slab and achieves uniform cooling and quality improvement of the slab.

CN118357428BActive Publication Date: 2026-11-24GANSU JIU STEEL GRP HONGXING IRON & STEEL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410579739.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-11
Publication Date
2026-11-24
Estimated Expiration
2044-05-11

AI Technical Summary

Technical Problem

In the continuous casting process of thick slabs, the problems of surface longitudinal cracks and steel leakage caused by local overcooling of the inner arc surface are difficult to solve effectively, and the existing technology is difficult to achieve uniform cooling in actual production.

Method used

In the secondary cooling zone of the slab continuous casting machine, the last inner arc support roller of each section is replaced with a straight roller, and air jet holes are set at both ends of it. High-pressure gas is used to spray out the collected secondary cooling water to avoid local overcooling of the inner arc surface.

Benefits of technology

This method achieves uniform cooling of the inner arc surface of the billet, reduces the incidence of surface longitudinal cracks, and improves product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118357428B_ABST
    Figure CN118357428B_ABST
Patent Text Reader

Abstract

The application discloses a system and method for relieving local supercooling of an inner arc surface of a wide-thick slab, and belongs to the technical field of metallurgy. The last support roller of the inner arc of each section of the secondary cooling zone of a wide-thick slab continuous casting machine is designed as a straight roller, air injection holes are arranged at positions 50-60 mm away from the top end of the two ends of the straight roller, the air injection holes are at an angle of 45 degrees with the roller surface, when the contact angle area between the straight roller and the inner arc of the cast slab is filled with water, the water will flow to the two ends along the contact angle, and when the water flows to the nozzle position, the water is high-speed injected away from the surface of the cast slab by high-pressure gas, the water flow superposition strengthening cooling effect of the inner arc surface of the wide-thick slab is weakened, the local supercooling of the inner arc surface of the wide-thick slab is effectively relieved, the problem of surface longitudinal cracks caused by local supercooling of the inner arc surface is solved, and the problem of uniform cooling of the inner arc of the slab is realized in a true sense.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metallurgical technology, specifically relating to a system and method for alleviating localized overcooling on the inner arc surface of a thick slab. Background Technology

[0002] In recent years, market demand for heavy steel plates has increased, making continuous casting of heavy slabs a new development trend. Compared to conventional slabs, heavy slabs differ significantly not only in equipment but also in their processing characteristics. The large cross-section and long metallurgical length of heavy slabs in continuous casting result in lower casting speeds, making surface and corner cracks highly susceptible to occur. These factors are the main challenges hindering the continuous casting production of heavy slabs.

[0003] Based on theoretical research, steel exhibits a brittle range between 600-900℃, during which the high-temperature thermoplasticity of the slab surface decreases rapidly. If straightening is performed within this temperature range, surface transverse cracks and corner transverse cracks are likely to occur. Traditionally, this problem for conventional slabs is addressed by avoiding the brittle range during straightening, typically using methods above 900℃ or below 600℃. However, for continuous casting production of wide and thick slabs, neither of these methods is easily implemented. The casting speed for wide and thick slabs is relatively low, resulting in a longer surface cooling time, making high-temperature straightening difficult. Furthermore, the greater thickness of wide and thick slabs significantly increases the strength requirements of the straightening section during low-temperature straightening, further complicating the process. In actual production, a weak cooling mode is used for the secondary cooling of wide and thick slabs, gradually increasing the temperature before entering the straightening section.

[0004] In order to ensure the goal of a steady drop in billet temperature, the secondary cooling spray process for thick plates under low casting speed conditions must ensure that the water spray cooling intensity on the billet surface is comparable to the internal thermal conductivity of the billet; otherwise, overcooling or overheating is very likely to occur.

[0005] Under weak secondary cooling conditions, the surface temperature difference of thick slabs is not significant. However, on the inner arc surface of the continuously cast slab, after the secondary cooling water is sprayed onto the slab surface, it accumulates along the inner arc surface, causing an increase in local cooling intensity. Combined with the low casting speed, this amplifies the increase in local cooling intensity on the inner arc surface. With increased cooling intensity, the slab surface shrinks faster than other areas. When secondary cooling water is sprayed onto the inner arc surface, it is more likely to accumulate in this area. After repeated application, stress concentration occurs in this area, resulting in numerous surface longitudinal cracks, which significantly impacts product quality.

[0006] Chinese invention patent CN201410073981.2 discloses a secondary cooling process for improving the surface quality of extra-thick slabs, belonging to the field of steelmaking-continuous casting technology. At the moment the slab exits the crystallizer, its surface is rapidly cooled, then the internal heat of the slab is used to reheat the surface. After reheating, the surface is slowly cooled again. This process improves the high-temperature thermoplasticity of the slab surface, reducing the probability of surface transverse cracks and corner transverse cracks. By controlling the cooling process of the slab surface, the third brittle zone is eliminated, improving the high-temperature plasticity of the extra-thick slab surface and solving the defects of surface transverse cracks and corner transverse cracks that easily occur during the production of extra-thick slabs. The advantages are that the process is relatively simple, widely applicable, and suitable for continuous casting slabs with thicknesses ranging from 400 to 600 mm and widths ranging from 1600 to 3000 mm.

[0007] Chinese invention patent (202210185989.2) discloses a method for adjusting and controlling the secondary cooling water volume at the corner of a slab casting to address quality defects. The method includes: collecting and preprocessing the operating status parameters of relevant equipment in steel production; constructing a visual topology using the preprocessed operating status parameters; and establishing an optimization constraint model based on the visual topology and historical data to adjust and control the secondary cooling water volume at the corner of the slab casting to address quality defects. This invention effectively reduces overcooling at the corners of the casting, preventing the casting from falling into the th brittle zone during the 7th to 8th straightening stages, which could lead to transverse cracks at the corners. By controlling the water volume at the edge of the casting machine, this invention achieves stable control of the edge quality of pericrystalline carbon and microalloy steel grades on the slab, thereby improving the yield of high-quality steel after rolling.

[0008] Compared to traditional slab continuous casting methods, the method provided by the aforementioned patent achieves the effect of controlling surface transverse cracks and corner cracks by adjusting the secondary cooling process mechanism or the secondary cooling water volume, representing a significant improvement over conventional slab continuous casting. The method employed in the invention patent (201410073981.2) involves rapidly cooling the slab surface after exiting the crystallizer, followed by reheating, and then slow cooling. This improves the high-temperature thermoplasticity of the slab surface and reduces the probability of surface and corner transverse cracks. However, based on conventional continuous casting knowledge, this operation has significant limitations. Rapid cooling after exiting the crystallizer causes rapid shrinkage of the slab shell, resulting in stress concentration in the middle of the wide face of the slab, easily causing surface longitudinal cracks and even leakage in that area. While the implementation of this patented technology can theoretically solve the defects of surface and corner transverse cracks in thick slabs, it will significantly increase the generation of surface longitudinal cracks and leakage. The applicability of this patent in production is questionable. The invention patent (202210185989.2) uses a system to detect the equipment's operating status and predict trends. The predicted data is then used to determine the amount of secondary cooling water at the corner of the billet, preventing the billet from falling into the th brittle zone during the 7th-8th straightening process, which could lead to transverse cracks at the corner. Based on common knowledge of continuous casting production, the core theory of this patent is essentially real-time dynamic water distribution. While theoretically feasible, it is impractical in actual production when the equipment cannot achieve single-drainage nozzle control. Summary of the Invention

[0009] Based on the problems mentioned in the background art, this invention provides a system and method for alleviating local overcooling of the inner arc surface of a thick slab. The last support roller in each section of the secondary cooling zone is redesigned, using a straight roller. Air jet holes are installed at both ends of the straight roller, 50-60 mm from the top, at a 45° angle to the roller surface. When the area at the contact angle between the straight roller and the inner arc of the slab is filled with water, the water flows along the roller towards both ends. Accelerated by this device, the water flow is sprayed towards both ends at a relatively high speed, effectively reducing the superimposed cooling effect of the water flow on the inner arc surface of the thick slab, effectively alleviating local overcooling of the inner arc surface of the slab, and solving the problem of surface longitudinal cracks caused by local overcooling of the inner arc surface. This truly achieves uniform cooling of the inner arc of the slab.

[0010] Therefore, the present invention adopts the following technical solution: A system for alleviating localized overcooling on the inner arc surface of a thick slab, wherein the last inner arc support roller of each section in the secondary cooling zone of a slab continuous casting machine is a straight roller, and a roller sleeve is provided on the straight roller; air jet holes are densely arranged at a distance of 50-60mm from the end of the roller sleeve at both ends, and each air jet hole is arranged at an equal angle along the circumference of the roller sleeve and penetrates the roller sleeve; it also includes an annular slide rail provided on the inner wall of the roller sleeve, the annular slide rail is arranged along the axis path of the air jet holes, and each air jet hole is located in the annular slide rail; It also includes a sliding sleeve, which is slidably connected to the annular slide rail and has an air intake pipe connected to it. When the straight roller rotates, the sliding sleeve connects to each jet hole in sequence, and the compressed air in the air intake pipe is discharged from the jet hole after passing through the sliding sleeve.

[0011] Furthermore, the jet holes are arranged at an angle, with the jet hole outlets facing the end of the roller sleeve, and the angle of inclination is 30° to 60°.

[0012] A method for alleviating localized undercooling on the inner arc surface of a thick slab includes the following steps: Step a. Replace the last inner arc support roller in each section of the secondary cooling zone of the slab continuous casting machine with a straight roller. Before production, complete the equipment debugging according to the arc calibration requirements. Step b. According to the corresponding steel grade produced by slab continuous casting, after the casting speed of the first furnace is normal, adjust the pressure in the air inlet pipe and control the air pressure according to the corresponding cooling mode; Step c. After the cooling water in each section of the inner arc is collected, it flows down along the inner arc surface of the billet. Under the action of the segmented support rollers in each section of the secondary cooling zone, the secondary cooling water is collected into streams and flows down. When the streams flow to the straight roller, the collected secondary cooling water flows along the channel formed by the billet and the straight roller towards the narrow surface of the billet, thus avoiding the superimposed cooling effect caused by the collection of secondary cooling water in the entire inner arc. Step d. When the secondary cooling water flows along the channel formed by the straight roller and the billet to the position of the air jet hole, the high-pressure gas ejected from the air jet hole meets the horizontally flowing secondary cooling water. Under the action of the high-pressure gas, the secondary cooling water is ejected at high speed. The spray distance is greater than the distance from the air jet hole to the narrow face of the billet. The secondary cooling water is directly blown away from the billet, avoiding the overcooling of the inner arc of the billet caused by the accumulation and superposition of the secondary cooling water.

[0013] The beneficial effects of this invention are as follows: 1. This invention solves the technical problem of local overcooling caused by the accumulation and superposition of the second cooling water in each section of the secondary cooling zone of the thick slab by designing the last inner arc support roller of each section of the secondary cooling zone as a straight roller and using the angle formed between the straight roller and the surface of the slab. 2. This invention redesigns the straight roller by setting air jet holes at both ends of the straight roller at a distance of 50-60mm from the top, with the air jet holes at a 45° angle to the roller surface. High-pressure gas is used to spray the water between the billet and the straight roller out of the billet surface, avoiding the water from the secondary cooling water from flowing down along the corners of the billet after it collects and flows out naturally, causing overcooling at the corners of the billet. This solves the technical problem of local overcooling caused by the collection of secondary cooling water on the inner arc surface, and effectively controls the billet quality defects caused by this. 3. This invention, by reasonably setting the spacing between the air nozzles on the roller surface and the width of the inner cavity of the sliding sleeve, and fixing the position of the sliding sleeve axis on the line connecting the center of the straight roller and the contact point of the casting billet, ensures that during the rotation of the optimized straight roller, when each nozzle rotates to this position, it forms a channel with the compressed air intake pipe through the sliding sleeve. Under the action of gas pressure, the water collected in the angle formed by the casting billet and the roller surface is sprayed away from the casting billet, solving the technical problem of water flowing down the corner after natural outflow, causing the corner to be too cold. Attached Figure Description

[0014] Figure 1 This is a comparison diagram of the roller system before and after the improvement of the present invention; Figure 2 This is a schematic diagram of the straight roller structure of the present invention; Figure 3 This is a schematic cross-sectional view of the straight roller AA of the present invention; In the diagram, 1-straight roller, 2-air jet hole, 3-roller sleeve, 4-sliding sleeve, 5-slide rail, 6-air inlet pipe, 7-pressure regulating valve. Detailed Implementation

[0015] The technical solution of the present invention will be described below with reference to the accompanying drawings and implementation methods.

[0016] Example 1: A system and method for alleviating localized undercooling on the inner arc surface of a thick slab, comprising the following steps: Step a. Replace the last inner arc support roller in each section of the secondary cooling zone of the slab continuous casting machine with straight roller 1. Before production, complete the equipment debugging according to the normal arc calibration requirements.

[0017] Step b. After the first furnace of Q235 is produced by continuous casting of slabs and the casting speed is normal, open the pressure regulating valve 7 on the air inlet pipe 6 and control the pressure according to the matching strong cooling mode of 1.0~1.2Mpa.

[0018] Step c. The cooling water in each section of the secondary cooling zone flows down along the inner arc of the billet after it is collected. With the action of the segmented support rollers of each secondary cooling zone, the secondary cooling water is collected into streams and flows down. When the collected streams flow to the straight roller 1, the collected secondary cooling water flows towards the narrow face of the billet along the channel formed by the billet and the straight roller 1.

[0019] Step d. When the secondary cooling water flows along the channel formed by the straight roller 1 and the billet to the position of the air jet hole 2, the high-pressure gas ejected from the air jet hole 2 meets the horizontally flowing secondary cooling water at a 45° angle. Under the action of the high-pressure gas, the secondary cooling water is ejected at high speed, with a spray distance of 80-110mm, which is greater than the distance from the air jet hole 2 to the narrow surface of the billet. The secondary cooling water is directly blown away from the billet, avoiding the overcooling of the inner arc of the billet caused by the accumulation and superposition of the secondary cooling water.

[0020] Step e. Use an infrared thermometer to measure the horizontal temperature distribution of the billet before it enters the straightening section. The specific temperature distribution is shown in the table below: Table 1 - Comparison of distribution changes before and after process optimization Location Left corner The midpoint of the angle Central The midpoint of the angle Right corner Temperature before optimization 911 935 952 917 902 Optimized temperature 906 921 933 925 907 Temperature monitoring revealed a more reasonable temperature distribution in the continuously cast billet before entering the straightening machine, with greater symmetry on both sides of the inner arc centerline, indicating better uniformity in the cooling process. Interim data analysis showed that the proportion of longitudinal cracks on the surface of the continuously cast billet decreased from 3.8‰ to 1.7‰ after process optimization, effectively solving the technical problem of localized overcooling caused by the accumulation of secondary cooling water on the inner arc surface, thus improving product quality.

[0021] Example 2: Step a. Replace the last inner arc support roller in each section of the secondary cooling zone of the slab continuous casting machine with straight roller 1. Before production, complete the equipment debugging according to the normal arc calibration requirements.

[0022] Step b. After the first furnace of 355E slab is cast and the casting speed is normal, open the pressure regulating valve 7 on the air inlet pipe 6 and control the pressure according to the matching weak cooling mode of 0.7~0.9Mpa.

[0023] Step c. The cooling water in each section of the secondary cooling zone flows down along the inner arc of the billet after it is collected. With the action of the segmented support rollers of each secondary cooling zone, the secondary cooling water is collected into streams and flows down. When the collected streams flow to the straight roller 1, the collected secondary cooling water flows towards the narrow face of the billet along the channel formed by the billet and the straight roller 1.

[0024] Step d. When the secondary cooling water flows along the channel formed by the straight roller 1 and the billet to the position of the air jet hole 2, the high-pressure gas ejected from the air jet hole 2 meets the horizontally flowing secondary cooling water at a 45° angle. Under the action of the high-pressure gas, the secondary cooling water is ejected at high speed, with a spray distance of 70-100mm, which is greater than the distance from the air jet hole 2 to the narrow surface of the billet. The secondary cooling water is directly blown away from the billet, avoiding the overcooling of the inner arc of the billet caused by the accumulation and superposition of the secondary cooling water.

[0025] Step e. Use an infrared thermometer to measure the horizontal temperature distribution of the billet before it enters the straightening section. The specific temperature distribution is shown in the table below: Table 2 - Comparison of distribution changes before and after process optimization Location Left corner The midpoint of the angle Central The midpoint of the angle Right corner Temperature before optimization 913 921 943 938 907 Optimized temperature 906 917 931 920 910 Temperature monitoring revealed a more reasonable temperature distribution in the continuously cast billet before entering the straightening machine, with greater symmetry on both sides of the inner arc centerline, indicating better uniformity in the cooling process. Interim data analysis showed that the proportion of longitudinal cracks on the surface of the continuously cast billet decreased from 2.9‰ to 1.3‰ after process optimization, effectively solving the technical problem of localized overcooling caused by the accumulation of secondary cooling water on the inner arc surface, thus improving product quality.

Claims

1. A system for alleviating localized undercooling on the inner arc surface of a thick slab, characterized in that, The last inner arc support roller of each section of the secondary cooling zone of the slab continuous casting machine is a straight roller (1), and a roller sleeve (3) is provided on the straight roller (1); air jet holes (2) are densely arranged at the left and right ends of the roller sleeve (3) at a distance of 50-60mm from the end, and each air jet hole (2) is arranged at an equal angle along the circumference of the roller sleeve (3), and the air jet hole (2) penetrates the roller sleeve (3); it also includes an annular slide (5) provided on the inner wall of the roller sleeve (3), the annular slide (5) is arranged along the axial path of the air jet hole (2), and each air jet hole (2) is located in the annular slide (5); It also includes a sliding sleeve (4), which is slidably connected to the annular slide (5). An air intake pipe (6) is connected to the sliding sleeve (4). When the straight roller (1) rotates, the sliding sleeve (4) connects to each jet hole (2) in sequence. The compressed air in the air intake pipe (6) is discharged from the jet hole (2) after passing through the sliding sleeve (4).

2. The system for alleviating localized overcooling on the inner arc surface of a thick slab according to claim 1, characterized in that, The jet holes (2) are arranged at an angle, with the outlet of the jet holes (2) facing the end of the roller sleeve (3), and the angle of inclination is 30° to 60°.

3. A method for alleviating localized undercooling on the inner arc surface of a thick slab, characterized in that, The system for alleviating localized overcooling on the inner arc surface of a thick slab, as described in any of claims 1-2, comprises the following specific steps: Step a. Replace the last inner arc support roller of each section in the secondary cooling zone of the slab continuous casting machine with a straight roller (1). Before production, complete the equipment debugging according to the arc calibration requirements. Step b. According to the corresponding steel grade produced by slab continuous casting, after the casting speed of the first furnace is normal, adjust the pressure in the air inlet pipe (6) and control the air pressure according to the corresponding cooling mode; Step c. After the cooling water in each section of the inner arc is collected, it flows down along the inner arc surface of the billet. Under the action of the segmented support rollers in each section of the secondary cooling zone, the secondary cooling water is collected into streams and flows down. When the streams flow to the straight roller (1), the collected secondary cooling water flows along the channel formed by the billet and the straight roller (1) towards the narrow surface of the billet, thus avoiding the superimposed cooling effect of the secondary cooling water in the entire inner arc being collected. Step d. When the secondary cooling water flows along the channel formed by the straight roller (1) and the billet to the position of the air jet hole (2), the high-pressure gas ejected from the air jet hole (2) meets the horizontally flowing secondary cooling water. Under the action of the high-pressure gas, the secondary cooling water is ejected at high speed. The ejection distance is greater than the distance from the air jet hole (2) to the narrow surface of the billet. The secondary cooling water is directly blown away from the billet, avoiding the overcooling of the inner arc of the billet caused by the accumulation and superposition of the secondary cooling water.

Citation Information

Patent Citations

  • Secondary cooling process for improving surface quality of extra-thick slab

    CN103846401B

  • Method for adjusting and controlling secondary cooling water quantity of edge with quality defect at corner of slab casting blank

    CN114653916A

  • Double-cooling section cooling water blowing apparatus for special-shaped blank continuous casting and uses method

    CN101367118A

  • Conticaster secondary cooling water sprays width control device

    CN207479552U