A radial gradient index infrared chalcogenide glass ceramic lens and a preparation method thereof
By fabricating a chalcogenide glass-ceramic lens composed of 65GeS₂-25In₂S₃-10CsCl, and employing a multi-temperature gradient furnace method to precipitate In₂S₃ nanocrystals in the central region of the lens, the problem of the lack of radial gradient refractive index materials in infrared imaging systems was solved, achieving a high-performance and lightweight infrared optical design.
Patent Information
- Application Number
- CN202410433826.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-11
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-04-11
AI Technical Summary
In existing infrared imaging systems, traditional lenses are difficult to integrate and lightweight, and there is a lack of radial gradient refractive index materials suitable for the infrared band, which makes it impossible to meet the requirements of high-performance optical design.
Chalcogenide glass ceramics composed of 65GeS₂-25In₂S₃-10CsCl were prepared by a multi-temperature gradient furnace method, in which In₂S₃ nanocrystals were precipitated in the middle region of the lens. The crystallinity decreased from the center to the edge, forming a high radial gradient refractive index difference, with the maximum refractive index difference Δn reaching more than 0.1.
A high-transparency radial gradient refractive index infrared chalcogenide glass-ceramic lens has been developed, suitable for miniaturized and lightweight infrared optical systems. It features a high radial gradient refractive index difference and is suitable for high-performance infrared optical materials in the visible and infrared ranges.
Smart Images

Figure CN118359381B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of infrared glass-ceramic materials technology, specifically to a radially gradient refractive index infrared chalcogenide glass-ceramic lens and its preparation method. Background Technology
[0002] To meet the needs of various fields, infrared optical systems require a balance between cost, performance, complexity, size, and weight (SWaP-C), making integration, miniaturization, and lightweighting inevitable trends. However, traditional infrared imaging systems consist of expensive non-planar lenses and complex lens assemblies, making integrated and lightweight designs difficult to achieve. Furthermore, while the development of advanced infrared focal plane array (FPA) detectors is progressing rapidly, the development of infrared lens materials is lagging significantly. Current FPA technology achieves pixel sizes as small as micrometers (5μm), and the design standards for infrared optics have reached the diffraction limit. Therefore, lenses with a single refractive index are no longer sufficient, making the development of novel optical lens imaging materials imperative.
[0003] Gradient-index (GRIN) lenses are optical devices with a spatially varying refractive index. When combined with refraction from the surface of the optics, the internal gradient refractive index characteristics provide optical designers with additional degrees of freedom, including providing additional thermal or chromatic aberration correction and achieving the SWaP-C target. Based on the different characteristics of the refractive index gradient distribution, gradient refractive index materials can be mainly divided into: axial gradient refractive index, radial gradient refractive index, and spherical gradient refractive index materials, among which radial GRIN materials are more ideal for optical design. Some gradient refractive index materials have been commercialized and successfully applied in products including optical couplers, collimators, and medical endoscopes. However, these products mainly operate in the visible light band, and there are no commercially available infrared gradient refractive index lens materials. In 2008, the U.S. Defense Advanced Research Projects Agency (DARPA) proposed the "M-GRIN" project for infrared GRIN materials; the European Union also included research on infrared GRIN glass materials in its "Horizon 2020" research and innovation framework program, making the application of chalcogenide glasses in infrared GRINs a focus of great attention.
[0004] Chalcogenide glasses are highly favored in the study of infrared gradient refractive index materials, representing a novel type of infrared optical material. Compared to other commonly used infrared materials, chalcogenide glasses possess advantages such as an excellent infrared transmission range (0.5-20 μm), strong glass-form capability, high chemical stability, simple preparation, ease of molding, and the ability to adjust composition to obtain desired optical properties. Studies have shown that heat treatment of chalcogenide glasses to obtain chalcogenide glass ceramics can improve chemical stability while altering optical properties (transmission window, refractive index). Furthermore, some chalcogenide glass ceramics can achieve controllable crystallization, allowing for the regulation of their optical properties through parameters such as crystal size and crystallinity.
[0005] Space temperature-controlled crystallization refers to the process of inducing the precipitation of high or low refractive index nanocrystals in a chalcogenide glass matrix through space-selective crystallization treatment, controlling the spatial distribution of nanocrystals to generate an effective refractive index gradient, and obtaining gradient refractive index structure materials. KANG et al. from the University of Central Florida [KANG M, SISKEN L, LONERGAN C, et al. Monolithic chalcogenide optical nanocomposites enable infrared system innovation: gradient refractive index optics[J]. Advanced Optical Materials, 2020, 8(10): 2000-150.] studied (Ge 30 As 10 Se 60 ) 1-xThe PbSex system was studied by subjecting a 5cm long 20GeSe2-60As2Se3-20PbSe glass rod to nucleation heat treatment at 220℃ for 2 hours. The rod was then placed along its axial direction in a temperature gradient furnace (temperature field 225℃-260℃) for 30 minutes, achieving axial GRIN with a refractive index gradient Δn = 0.15@5μm. Thomas et al. from the University of Rennes 1, France [LAVANANT E, CALVEZ L, CHEVIRé F, et al. Radial gradient refractive index (GRIN) infrared lens based on spatially resolved crystallization of chalcogenide glass[J]. Optical Materials Express, 2020, 10(4): 860-867.] used ring heating, slowly passing a chalcogenide glass rod through a heating ring at a speed of 0.6mm / min. The low thermal conductivity of chalcogenide glass materials prevents the formation of a uniform temperature field inside the glass, resulting in a radial temperature distribution, thus achieving a radial distribution of crystallization and refractive index. This method achieves crystallization at the edge of an 80GeSe2–20Ga2Se3 glass rod, with a gradient decrease towards the center, yielding a maximum refractive index difference of Δn = 0.03 @ 10 μm. Therefore, the space-temperature controlled crystallization method shows great potential for fabricating axial and radial GRINs. However, research on radial GRIN infrared chalcogenide glass lenses, which are more suitable for optical design, remains limited, and the maximum refractive index difference of Δn = 0.03 is far from meeting commercialization requirements. Summary of the Invention
[0006] The technical problem to be solved by the present invention is to provide a radial gradient refractive index infrared chalcogenide glass-ceramic lens and its preparation method, which addresses the shortcomings of the prior art. This lens can achieve a high radial gradient refractive index difference, with a maximum refractive index difference Δn of more than 0.1 at the 5.78μm band. It has high transparency in the visible and infrared range (0.5~12μm) and is a novel infrared optical material with a high radial gradient refractive index. It has great potential for application in miniaturized, lightweight and high-performance infrared optical systems.
[0007] The technical solution adopted by the present invention to solve the above-mentioned technical problems is as follows: a radial gradient refractive index infrared chalcogenide glass-ceramic lens, the lens being made of chalcogenide glass-ceramic, the molar composition of which is expressed by the chemical formula 65GeS2-25In2S3-10CsCl, the lens containing In2S3 nanocrystals, the lens precipitating In2S3 nanocrystals only in the middle region, and in the radial direction of the lens, the crystallinity of the precipitated In2S3 nanocrystals decreases in a gradient from the center of the middle region to the edge of the middle region.
[0008] The method for fabricating the above-mentioned radial gradient refractive index infrared chalcogenide glass-ceramic lens includes the following steps:
[0009] (1) Based on the composition of chalcogenide glass ceramics, calculate the required amount of each element, weigh the high-purity germanium, indium, sulfur, and cesium chloride raw materials, and control the error within ±0.001g. Then, slowly pour the raw materials into a dry and clean quartz tube, and evacuate the quartz tube to 10°C. -4 Pa, encapsulates the raw materials in a quartz tube;
[0010] (2) Place the quartz tube into the swing furnace and melt the raw material at a high temperature of 900-980℃ for 12-25 hours. After melting, remove the quartz tube from the swing furnace and immerse it in ice water or quench it with compressed air. Remove the quartz tube immediately after the wall is removed.
[0011] (3) Quickly place the quartz tube into the annealing furnace and keep it warm. The annealing temperature is 280-320℃ and the annealing time is 6h. After the annealing is completed, cool it down to room temperature at a cooling rate of 9-10℃ / h. Open the quartz tube to obtain the 65GeS2-25In2S3-10CsCl basic chalcogenide glass sample. Grind the sample into a glass rod.
[0012] (4) Prepare a multi-temperature gradient furnace, which includes a lifting platform and three furnace chambers that can be independently temperature controlled and are sealed. The three furnace chambers are arranged vertically and connected to each other. The three furnace chambers are connected to a vent pipe. The lifting platform can move up and down within the three furnace chambers.
[0013] First, set the target temperatures for the upper, middle, and lower furnace chambers according to high, medium, and low temperatures respectively, and ensure that the target temperatures of the three furnace chambers exceed the glass transition temperature of 65GeS2-25In2S3-10CsCl chalcogenide glass. The upper, middle, and lower furnace chambers are designated as three constant temperature zones: a high-temperature zone, a medium-temperature zone, and a low-temperature zone. Set the moving speed of the lifting platform. Second, vertically fix the glass rod obtained in step (3) on the lifting platform, start the lifting platform to move the glass rod to the high-temperature zone, and then close the lifting platform. Then, turn on the multi-temperature gradient furnace and introduce nitrogen gas into the three furnace chambers through the vent pipe. The three furnace chambers were heated to the target temperature at the same heating rate. When the temperature of the high-temperature zone reached the target temperature, the lifting platform was activated, which moved the glass rod to the medium-temperature zone and the low-temperature zone at a constant speed, and then to the high-temperature zone. This process was repeated multiple times to perform gradient crystallization heat treatment, resulting in the precipitation of In2S3 nanocrystals with a radial gradient distribution in the middle of the glass rod. Finally, the multi-temperature gradient furnace and the lifting platform were turned off, and the nitrogen gas supply to the three furnace chambers was stopped. After the furnace chambers cooled naturally to room temperature, the glass rod was removed, sliced, ground, and polished into a lens, thus obtaining a radially gradient refractive index infrared chalcogenide glass-ceramic lens.
[0014] During the gradient crystallization heat treatment, the lifting platform reciprocates between three constant temperature zones: high temperature, medium temperature, and low temperature. The low thermal conductivity of the 65GeS2-25In2S3-10CsCl glass rod, combined with the stretching motion, prevents the formation of a uniform temperature field inside the glass rod. In particular, the heat scattering at the edge of the glass rod is accelerated from the high temperature zone to the low temperature zone, resulting in a higher temperature in the middle region of the glass rod and a lower temperature at the edge region, forming the required radial gradient temperature distribution and precipitating In2S3 nanocrystals with a radial gradient distribution.
[0015] Preferably, the germanium, indium, and sulfur used in step (1) are all 5N in purity, and the cesium chloride is 4N in purity, so as to ensure the purity and composition uniformity of the obtained chalcogenide glass ceramic material.
[0016] Preferably, in step (4), the target temperature values of the upper, middle and lower furnace chambers are set as a, b and c respectively, and the value ranges of a, b and c are: 380℃<a≤400℃, 360℃<b≤380℃, 340℃<c≤360℃ respectively. The heating rate of the three furnace chambers is 0.5~2℃ / min, the constant moving speed of the lifting platform is 40~70mm / min, and the moving time of the lifting platform is 10~15h.
[0017] Preferably, within the heat treatment temperature range of 370–400 °C, the strength of the In2S3 nanocrystals precipitated in the chalcogenide glass ceramic 65GeS2-25In2S3-10CsCl increases with increasing heat treatment temperature, and the refractive index of the chalcogenide glass ceramic is positively correlated with the strength of the precipitated In2S3 nanocrystals.
[0018] Compared with the prior art, the present invention has the following advantages:
[0019] (1) The radial gradient refractive index infrared chalcogenide glass-ceramic lens of the present invention is made of environmentally friendly raw materials, consisting of chalcogenide glass-ceramics with a molar composition of 65GeS2-25In2S3-10CsCl, and does not contain elements with strong environmental toxicity such as arsenic and lead. The lens contains In2S3 nanocrystals, which have high transparency in the visible and infrared range (0.5-12μm), with a transmittance of >60% in the 2.5-12μm infrared band, and is also transparent in the visible light range. The lens precipitates In2S3 nanocrystals only in the middle region, and the crystallinity of the precipitated In2S3 nanocrystals decreases in a gradient from the center to the edge of the middle region in the radial direction of the lens, which can achieve a high radial gradient refractive index difference. The maximum refractive index difference Δn at the 5.78μm band can reach more than 0.1. It is a new type of infrared optical material with a high radial gradient refractive index and has great potential for application in infrared optical systems such as miniaturized, lightweight and high-performance infrared thermal imagers.
[0020] (2) The method for preparing the radial gradient refractive index infrared chalcogenide glass-ceramic lens of the present invention achieves radial gradient precipitation of In2S3 nanocrystals by creating a radial spatial gradient temperature field and controlling crystallization through multiple temperature fields. This invention is the first to successfully achieve crystallization in the internal region of a glass rod while simultaneously realizing radial gradient decay diffusion. The method of the present invention for preparing radial gradient refractive index infrared chalcogenide glass-ceramic lenses is characterized by short preparation time, simple operation, high efficiency, and significant industrialization value. Attached Figure Description
[0021] Figure 1 This is a simplified structural diagram of the multi-temperature gradient furnace used in Example 1;
[0022] Figure 2 This is a photograph of the radial gradient refractive index infrared chalcogenide glass-ceramic lens prepared in Example 1.
[0023] Figure 3 Infrared spectra at different locations on the cross-section of the radial gradient refractive index infrared chalcogenide glass-ceramic lens prepared in Example 1;
[0024] Figure 4 The image shows the refractive index distribution of the radial gradient refractive index infrared chalcogenide glass-ceramic lens prepared in Example 1. Detailed Implementation
[0025] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments.
[0026] Example 1: A radially gradient refractive index infrared chalcogenide glass-ceramic lens, made of chalcogenide glass-ceramic with a molar composition expressed by the chemical formula 65GeS2-25In2S3-10CsCl. The lens contains In2S3 nanocrystals, which are precipitated only in the central region. Furthermore, the crystallinity of the precipitated In2S3 nanocrystals decreases gradually from the center to the edge of the central region along the radial direction of the lens. The preparation method of this lens includes the following steps:
[0027] (1) Based on the composition of chalcogenide glass ceramics, calculate the required amount of each element. Weigh germanium, indium, sulfur (purity 5N) and cesium chloride (purity 4N) raw materials, and control the error within ±0.001g. Prepare a quartz tube with an inner diameter of 10mm, soak the quartz tube in aqua regia for 2 hours, wash it with distilled water, and dry it. Then slowly pour the raw materials into the quartz tube and evacuate the quartz tube to 10 ... -4 Pa, and then the quartz tube was sealed with a hydrogen-oxygen flame;
[0028] (2) Place the quartz tube into the swing furnace and melt the raw material at a high temperature of 980°C. After melting for 25 hours, take the quartz tube out of the swing furnace and immerse it in ice water to quench it. Once the wall is broken off, take the quartz tube out immediately.
[0029] (3) Quickly place the quartz tube into the annealing furnace and keep it at 300℃ for 6 hours. After annealing, cool it down to room temperature at a rate of 10℃ / h. Open the quartz tube to obtain a 65GeS2-25In2S3-10CsCl basic chalcogenide glass sample. Grind the sample into a glass rod with a diameter of 10mm and a length of 50mm.
[0030] (4) Prepare a multi-temperature gradient furnace, such as Figure 1 As shown, the multi-temperature gradient furnace includes a lifting platform 4 and three independently temperature-controlled and sealed furnace chambers 1, 2, and 3. The three furnace chambers 1, 2, and 3 are set on the base 6. The three furnace chambers 1, 2, and 3 are arranged vertically and connected to each other. The height of the three furnace chambers 1, 2, and 3 is 10cm. The three furnace chambers 1, 2, and 3 are connected to a vent pipe 5. The lifting platform 4 can move up and down inside the three furnace chambers 1, 2, and 3.
[0031] First, set the target temperatures of the upper, middle, and lower furnace chambers 1, 2, and 3 according to high, medium, and low temperatures respectively. The target temperatures of the three furnace chambers 1, 2, and 3 should exceed the glass transition temperature of 65GeS2-25In2S3-10CsCl chalcogenide glass. The upper, middle, and lower furnace chambers 1, 2, and 3 are designated as three constant temperature zones, namely, the high temperature zone, the medium temperature zone, and the low temperature zone. The target temperature values of the upper, middle, and lower furnace chambers 1, 2, and 3 are recorded as a, b, and c respectively, with values of 390℃, 375℃, and 360℃ respectively. The moving speed of the lifting platform 4 is also set. Second, fix the glass rod 7 obtained in step (3) vertically on the lifting platform 4, start the lifting platform 4 to move the glass rod 7 to the high temperature zone, and then turn off the lifting platform 4. Then, turn on the multi-temperature gradient furnace and introduce nitrogen gas into the three furnace chambers 1, 2, and 3 through the gas pipe 5. The function is to prevent oxidation of the glass rod surface. The three furnace chambers 1, 2, and 3 are slowly heated to the target temperature at the same heating rate of 2℃ / min. Once the high-temperature zone reaches the target temperature, the lifting platform 4 is activated, moving the glass rod 7 at a constant speed of 60mm / min to the medium-temperature zone and then the low-temperature zone, before moving it back to the high-temperature zone. This process is repeated multiple times (the cumulative moving time of the lifting platform 4 is 12 hours) to perform gradient crystallization heat treatment, precipitating In2S3 nanocrystals with a radial gradient distribution in the middle of the glass rod 7. Finally, the multi-temperature gradient furnace and the lifting platform 4 are shut down, and nitrogen gas is stopped being introduced into the three furnace chambers 1, 2, and 3. After the furnace chambers cool naturally to room temperature, the glass rod 7 is removed, sliced, ground, and polished into lenses with a thickness of 1.5–2.5mm and a diameter of 10mm, thus obtaining a radially gradient refractive index infrared chalcogenide glass-ceramic lens. Figure 2 As shown in the figure, the darker circular central area is the crystallization region of In2S3 nanocrystals. The lens precipitates In2S3 nanocrystals only in the central area, and the crystallinity of the precipitated In2S3 nanocrystals decreases in a gradient from the center of the central area to the edge of the central area in the radial direction of the lens.
[0032] On the lens obtained in Example 1, from the edge of the lens ( Figure 3 The edge of the crystallization region of In2S3 nanocrystals (marked as "edge-1"). Figure 3 The center of the crystallization region of In2S3 nanocrystals (marked as "edge-2") and the region marked as "edge-2" in the middle) Figure 3 Points were taken from the middle (marked as "middle-3") and tested on a Fourier transform infrared spectrometer. The infrared spectra are shown below. Figure 3 The results showed that the lens maintained good transmittance in the 2.5–12.5 μm infrared band, and the infrared transmittance decreased sequentially from the edge of the lens toward the center of the crystallization region of the In2S3 nanocrystals, indicating that the In2S3 nanocrystals grew in a gradient inside the lens.
[0033] The refractive index of the center and edge of the crystallization region of the In2S3 nanocrystal in the lens prepared in Example 1 was measured using an infrared ellipsometer. A confocal Raman spectroscopy was used to perform a radial scan of the crystallization region of the In2S3 nanocrystal towards the edge to characterize the refractive index distribution inside the lens. Figure 4 The refractive index distribution diagram shown indicates that the test results show that the maximum refractive index span Δn of the fabricated lens in the 5.78μm band can reach more than 0.1.
Claims
1. A radially gradient refractive index infrared chalcogenide glass-ceramic lens, characterized in that, The lens is made of chalcogenide glass-ceramic with a molar composition expressed by the chemical formula 65GeS2-25In2S3-10CsCl. The lens contains In2S3 nanocrystals, which are precipitated only in the central region. Furthermore, the crystallinity of the precipitated In2S3 nanocrystals decreases gradually from the center to the edge of the central region along the radial direction of the lens. The refractive index of the central region is higher than that of the edge region. The maximum refractive index difference Δn at a wavelength of 5.78 μm is ≥0.1, and the transmittance in the 2.5–12 μm infrared band is >60%.
2. The method for preparing the radially gradient refractive index infrared chalcogenide glass-ceramic lens according to claim 1, characterized in that, Includes the following steps: (1) Based on the composition of chalcogenide glass ceramics, calculate the required amount of each element, weigh the high-purity germanium, indium, sulfur, and cesium chloride raw materials, and control the error within ±0.001g. Then, slowly pour the raw materials into a dry and clean quartz tube and evacuate the quartz tube to 10°C. -4 Pa, encapsulates the raw materials in a quartz tube; (2) Place the quartz tube into the swing furnace and melt the raw material at a high temperature of 900-980℃ for 12-25 hours. After melting, remove the quartz tube from the swing furnace and immerse it in ice water or quench it with compressed air. Remove the quartz tube immediately after the wall is removed. (3) Quickly place the quartz tube into the annealing furnace and keep it warm. The annealing temperature is 280-320℃ and the annealing time is 6h. After the annealing is completed, cool it down to room temperature at a cooling rate of 9-10℃ / h. Open the quartz tube to obtain the 65GeS2-25In2S3-10CsCl basic chalcogenide glass sample. Grind the sample into a glass rod. (4) Prepare a multi-temperature gradient furnace, which includes a lifting platform and three furnace chambers that can be independently temperature controlled and are sealed. The three furnace chambers are arranged vertically and connected to each other. The three furnace chambers are connected to a vent pipe. The lifting platform can move up and down within the three furnace chambers. First, set the target temperatures of the upper, middle, and lower furnace chambers according to three temperatures: high, medium, and low. The target temperatures of the three furnace chambers should exceed the glass transition temperature of 65GeS2-25In2S3-10CsCl chalcogenide glass. The upper, middle, and lower furnace chambers are designated as three constant temperature zones: high temperature zone, medium temperature zone, and low temperature zone. The target temperature values of the upper, middle, and lower furnace chambers are denoted as a, b, and c, respectively. The ranges of a, b, and c are: 380℃<a≤400℃, 360℃<b≤380℃, and 340℃<c≤360℃, respectively. The heating rate of the three furnace chambers is 0.5~2℃ / min, the constant moving speed of the lifting platform is 40~70mm / min, and the moving time of the lifting platform is 10~15h. Second, the glass rod obtained in step (3) is... The glass rod is vertically fixed on a lifting platform. The lifting platform is activated, moving the glass rod to the high-temperature zone, and then the lifting platform is closed. Next, a multi-temperature gradient furnace is turned on, and nitrogen is introduced into the three furnace chambers through the vent pipe. The three furnace chambers are heated to the target temperature at the same heating rate. When the temperature of the high-temperature zone reaches the target temperature, the lifting platform is activated, moving the glass rod to the medium-temperature zone and the low-temperature zone at a constant speed, and then to the high-temperature zone. This process is repeated multiple times to perform gradient crystallization heat treatment, precipitating In2S3 nanocrystals with a radial gradient distribution in the middle of the glass rod. Finally, the multi-temperature gradient furnace and the lifting platform are turned off, and the nitrogen supply to the three furnace chambers is stopped. The furnace chambers are allowed to cool naturally to room temperature. The glass rod is then removed, sliced, ground, and polished into a lens, thus obtaining a radially gradient refractive index infrared chalcogenide glass-ceramic lens.
3. The method for preparing a radially gradient refractive index infrared chalcogenide glass-ceramic lens according to claim 2, characterized in that, In step (1), the germanium, indium, and sulfur used are all 5N in purity, and the cesium chloride is 4N in purity.
4. The method for preparing a radially gradient refractive index infrared chalcogenide glass-ceramic lens according to claim 2, characterized in that, Within the heat treatment temperature range of 370–400 °C, the strength of the In2S3 nanocrystals precipitated in the chalcogenide glass ceramic 65GeS2-25In2S3-10CsCl increases with increasing heat treatment temperature, and the refractive index of the chalcogenide glass ceramic is positively correlated with the strength of the precipitated In2S3 nanocrystals.
Citation Information
Patent Citations
Sulfur-based glass-ceramic material and production method thereof