A composite coating liquid based on attapulgite modification and a preparation method thereof
By modifying attapulgite and mixing it with polyvinyl alcohol aqueous solution, a composite coating liquid was prepared and applied to paper, which solved the problem of insufficient barrier properties of packaging materials and achieved high-efficiency barrier properties and improved mechanical properties of paper.
Patent Information
- Application Number
- CN202410579160.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-11
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-05-11
AI Technical Summary
Existing packaging materials have insufficient barrier properties, making food and medicine prone to spoilage and unable to effectively prevent the penetration of oxygen, water vapor and organic solvents, thus affecting shelf life and expiration date.
By modifying attapulgite and heating it to mix with an aqueous solution of polyvinyl alcohol, a composite coating solution is prepared and applied to the surface of paper to form modified attapulgite/PVA barrier paper, which enhances the tensile strength, hydrophobicity and gas barrier properties of the paper.
It improves the tensile strength, hydrophobicity, and gas barrier properties of paper, significantly reduces air permeability, enhances the barrier effect against oxygen, water vapor, and organic solvents, and extends the shelf life of food and medicine.
Smart Images

Figure CN118360818B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of paper coating technology, specifically relating to a composite coating liquid based on attapulgite modification and its preparation method. Background Technology
[0002] The barrier properties of containers and packaging materials are defined as their ability to prevent the permeation of small molecule gases such as oxygen, carbon dioxide, water vapor, and other organic solvent vapors. High-barrier plastic packaging materials effectively block the permeation of oxygen and water vapor while retaining certain gaseous components within the packaging, thus significantly extending the shelf life and expiration date of various goods. Technically, barrier properties refer to a very low permeability to small molecular weight chemicals, such as gases and organic matter.
[0003] Currently, due to inadequate protective measures, large quantities of food are spoiling and deteriorating. Simultaneously, illness and death are resulting from consuming expired food and medications, all of which are largely related to the failure of barrier properties in packaging materials. Barrier properties are an essential function of packaging materials. In the food and pharmaceutical industries, the requirements for barrier properties are even higher. Packaging materials must prevent the penetration of oxygen, water vapor, and corrosive solvents such as acids and alkalis, as well as the leakage of organic vapors and aromas, to stabilize the internal environment of the packaging and protect the contents, thereby extending the shelf life and expiration period of pharmaceuticals, food, and other commodities.
[0004] Chinese patent application publication number CN 101914870 B discloses an aqueous coating for cigarette forming paper containing attapulgite. The aqueous coating adheres well to the forming paper, effectively ensuring the adsorption function of attapulgite to reduce harmful substances in cigarette smoke. There is no problem of volatile organic solvent residue after coating, saving energy, being safe and pollution-free, and making smoking safer. In addition, the carboxymethyl cellulose contained therein can enhance the strength of the paper. Summary of the Invention
[0005] To address the shortcomings of existing technologies, the present invention aims to provide a composite coating liquid based on attapulgite modification and its preparation method, thereby solving the aforementioned technical problems in the prior art.
[0006] The objective of this invention can be achieved through the following technical solutions: A composite coating liquid based on modified attapulgite includes modifying attapulgite and then heating and mixing it with an aqueous solution of polyvinyl alcohol to obtain the composite coating liquid. When this composite coating liquid is applied to paper, the tensile strength of the paper reaches more than 21.885 N·m / g; the water phase contact angle is 90.6° to obtain hydrophobicity, and the air permeability is increased to 1.27531 μm / Pa·s.
[0007] The preparation method of the composite coating liquid based on attapulgite modification includes the following steps: S1. First, take a sample of the modified liquid, then add attapulgite to mix, and obtain solution A; S2. Centrifuge the obtained solution A to separate the dilute hydrochloric acid from the surface of the attapulgite, and then wash, dehydrate and dry it to obtain modified attapulgite. S3. Subsequently, the modified attapulgite is placed in a polyvinyl alcohol aqueous solution (PVA solution) and heated and stirred in water at a constant temperature of 90°C to obtain a composite coating liquid.
[0008] Furthermore, in step S1, after adding attapulgite, the mixture is stirred for 6 hours to allow the modified liquid to form a sufficient reactive contact with the surface of the attapulgite.
[0009] Furthermore, in S1, the modifying solution is a 5 mol / L dilute hydrochloric acid solution or a 1 mol / L NaOH solution.
[0010] Furthermore, in S2, solution A is centrifuged at a high speed of 9500 r / min for at least 2 minutes.
[0011] Furthermore, the polyvinyl alcohol water content in S3 is 5g PVA / 95mL water by weight.
[0012] Furthermore, in S3, when heating at a constant temperature of 90°C, a water bath is used for heating.
[0013] Furthermore, the application of the composite coating liquid is as follows: the obtained composite coating liquid is coated on the surface of paper to form barrier paper, which is then dried to remove solvent and moisture, thereby obtaining modified attapulgite / PVA barrier paper.
[0014] The beneficial effects of this invention are: 1. In this invention, after modification with attapulgite, the silicon-oxygen-silicon bonds of the PVA successfully replaced the hydroxyl groups on the surface. The acid-treated attapulgite / PVA has a thickness of 1654.53 cm⁻¹. -1 The characteristic peak of the water of crystallization is stronger than that of other groups, indicating that PVA may have interacted with attapulgite through hydrogen bonds. Therefore, the modified acid treatment is more conducive to the composite with PVA.
[0015] 2. The acid-treated attapulgite / PVA barrier paper of this invention exhibits improved tensile strength, grease resistance, hydrophobicity, gas barrier properties, and oil absorption. Its tensile strength is 21.885 N·m / g, a 7.2% increase compared to the base paper. Grease resistance is significantly improved compared to the base paper, achieving a grease resistance grade of 7. The aqueous phase contact angle is 90.6°, exhibiting hydrophobicity compared to hydrophilic PVA barrier paper. The oil phase contact angle is 92.6°, demonstrating good oleophobicity compared to PVA barrier paper. It has the lowest air permeability at 1.27531 μm / Pa·s, even lower than that of 3010 coated paper. This represents a 59.30% decrease compared to the base paper and an 8.15% decrease compared to PVA barrier paper. Compared to both the base paper and PVA barrier paper, the COBB value of the 50mg acid-treated attapulgite / PVA barrier paper is significantly lower, indicating lower oil absorption. In summary, attapulgite / PVA barrier paper treated with 50mg acid not only has good barrier properties but also good mechanical properties.
[0016] 3. Compared with PVA barrier paper, the acid-treated attapulgite / PVA barrier paper used in this invention exhibits superior performance in all aspects. This is mainly due to the combined effects of attapulgite modification, PVA network reinforcement, enhanced attapulgite-PVA interface effect, optimized microstructure, and improved surface structure. These changes strengthen the internal interactions of the material, optimize its structure, and enhance its stability, thereby improving overall performance.
[0017] 4. The acid-treated attapulgite / PVA barrier paper used in this invention possesses excellent comprehensive performance and can be applied in a wide range of fields. It can be used alone as a barrier and protective material for various applications, or it can be compounded with other materials to achieve synergistic effects. The material itself can also be used as an additive and modifier for various polymer materials. Attached Figure Description
[0018] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below.
[0019] Figure 1 These are SEM (Scanning Electron Microscope) images of attapulgite and barrier paper according to an embodiment of the present invention. Figure 2 This is an infrared spectrum of acid-treated attapulgite / PVA according to an embodiment of the present invention; Figure 3 This is an infrared spectrum of alkali-treated attapulgite / PVA according to an embodiment of the present invention; Figure 4 This is a schematic diagram of the tensile strength of acid-treated attapulgite-modified PVA barrier paper according to an embodiment of the present invention. Figure 5This is a schematic diagram of the tensile strength of the alkali-treated attapulgite-modified PVA barrier paper according to an embodiment of the present invention. Figure 6 These are microscopic images of the acid-treated attapulgite-modified PVA barrier paper and the aqueous phase contact angle of the comparative example of the present invention. Figure 7 These are microscopic images of the alkali-treated attapulgite-modified PVA barrier paper and the aqueous phase contact angle of the comparative example of the present invention. Figure 8 These are microscopic images of the oil phase contact angle of acid-treated attapulgite-modified PVA barrier paper and alkali-treated attapulgite-modified PVA barrier paper in the embodiments and comparative examples of the present invention. Figure 9 This is a schematic diagram of the air permeability of acid-treated attapulgite-modified PVA barrier paper according to an embodiment of the present invention. Figure 10 This is a schematic diagram of the air permeability of the alkali-treated attapulgite-modified PVA barrier paper according to an embodiment of the present invention. Detailed Implementation
[0020] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0021] This invention provides a composite coating liquid based on modified attapulgite, comprising modifying attapulgite and then heating and mixing it with an aqueous solution of polyvinyl alcohol to obtain the composite coating liquid. When this composite coating liquid is applied to paper, the tensile strength of the paper reaches more than 21.885 N·m / g; the water phase contact angle is 90.6° to obtain hydrophobicity, and the air permeability is increased to 1.27531 μm / Pa·s.
[0022] The preparation method of the composite coating liquid based on attapulgite modification includes the following steps: S1. First, take a sample of the modified solution, then add attapulgite to the mixture and stir for 6 hours to allow the modified solution to form a sufficient reaction contact with the surface of the attapulgite, thus obtaining solution A; wherein the modified solution is a 5 mol / L dilute hydrochloric acid solution or a 1 mol / L NaOH solution.
[0023] S2. Centrifuge the obtained solution A (using a high speed of 9500 r / min for at least 2 min) to separate the dilute hydrochloric acid on the surface of the attapulgite. Then, wash, dehydrate, and dry the solution to obtain the modified attapulgite. S3. Subsequently, the modified attapulgite is placed in a polyvinyl alcohol aqueous solution (5g PVA / 95mL water by weight), and heated and stirred in a water bath at a constant temperature of 90℃ to obtain a composite coating liquid.
[0024] The specific plan is as follows: Acid-treated attapulgite-modified PVA coating Prepare 240 mL of 5 mol / L dilute hydrochloric acid solution by mixing 100 mol / L hydrochloric acid with 140 mL of water. Weigh 20 g of attapulgite and mix it with 200 mL of dilute hydrochloric acid, then stir magnetically for 6 hours. Pour the stirred solution into four centrifuge tubes and centrifuge at 9500 rpm for 2 minutes to separate the dilute hydrochloric acid adhering to the surface of the attapulgite. Wash with deionized water and centrifuge, repeating this process four times to remove excess water. Dry the acid-treated attapulgite, weighing it to 17.7145 g, and store it for later use.
[0025] Weigh 5g of PVA and mix with 95mL of water. Stir magnetically at 90°C in a constant temperature water bath. Set the prepared solution aside. Perform the same operation on 3010 coated paper (i.e., the experimental subject coated according to the method of this application). Weigh 5g of PVA and mix with 95mL of water, then weigh 25mg of acid-treated attapulgite, mix, and stir magnetically at 90°C in a constant temperature water bath. Set the prepared solution aside. Perform the same operation on 50mg, 100mg, 150mg, and 200mg of acid-treated attapulgite.
[0026] Alkali-treated attapulgite-modified PVA coating: Prepare a 1 mol / L NaOH solution by weighing 8 g of solid NaOH and 200 mL of water (slowly add the NaOH to a 250 mL beaker containing 200 mL of water while stirring with a glass rod to prevent the solid from settling at the bottom and becoming difficult to dissolve). Then, weigh 20 g of attapulgite and mix it with the NaOH solution, stirring magnetically for 6 hours. Next, pour the solution into four centrifuge tubes and centrifuge at 9500 rpm for 2 minutes to separate the NaOH adhering to the surface of the attapulgite. Wash with deionized water and centrifuge, repeating this process four times to remove excess water. Dry the alkali-treated attapulgite, weighing it to 19.5487 g, and store it for later use.
[0027] Weigh 5g of PVA and mix it with 95mL of water. Then weigh 25mg of alkali-treated attapulgite and mix them together. Stir the mixture magnetically in a constant temperature water bath at 90℃. Set the stirred solution aside. Similarly, perform the same operation on 25mg, 50mg, 100mg, 150mg, and 200mg of alkali-treated attapulgite.
[0028] Preparation of attapulgite-modified PVA barrier paper: At 70g / m2 Using A4 base paper as the base paper, the modified PVA coating solution prepared in each group was evenly coated on the paper surface to obtain barrier paper. The paper was dried in a paper sheet desiccator at 76°C to completely remove the solvent. After that, the barrier paper was placed in a constant temperature and humidity laboratory for more than 24 hours to balance the moisture.
[0029] Membrane preparation: Using different droppers, drop each group of solutions onto a petri dish and mark them. Then place the dish in a 60℃ vacuum drying oven to dry completely. After drying, remove the membrane and store it.
[0030] like Figure 1 As shown, the scanning results for attapulgite, acid / alkali treated attapulgite, and various barrier papers are as follows: Figure 1 As shown, by Figure 1 (a) It can be seen that untreated attapulgite is large in size and agglomerated; after acid treatment or alkali etching, the metal ions or Si-O-Si bonds between silicate crystals are replaced by H and OH, reducing the size of silicate particles. Further mixing with PVA solution on the paper surface will further fill the pores between cellulose particles. Figure 1 (f) uses acid-treated attapulgite mixed 1799 coated paper, and (g) uses alkali-treated attapulgite mixed 1799 coated paper.
[0031] Obvious features indicate that Figure 1 (e) That is, the fiber surface of 3010 coated paper has fewer pores and higher flatness.
[0032] The results of the infrared spectroscopy of acid-treated attapulgite / PVA are as follows: Figure 2 As shown (the order from 25mg acid to 3010 coated paper in the upper right corner corresponds to the top-to-bottom arrangement of the drawings), the figure shows that at 1085.42cm... -1 841.80cm -1 472.18cm -1 The same characteristic peak appeared in each group. 1085.42cm -1 This is a strong absorption peak in Si-O-Si, representing the most important and typical characteristic of silicon-oxygen-silicon bonds. 841.80 cm⁻¹ -1 It is the symmetrical bending vibration peak of Si-O-Si, at 472.18 cm⁻¹. -1 These are the bending vibration peaks of Si-O-Si. The appearance of these characteristic peaks proves the existence of silicon-oxygen-silicon bonds. Therefore, it can be seen that after PVA is modified with attapulgite, the Si-O-Si bonds successfully replace the hydroxyl groups on the surface. As shown in the figure, there is no significant difference in the characteristic peaks of attapulgite / PVA treated with different amounts of acid, but the peak at 1654.53 cm⁻¹ is significantly different after attapulgite / PVA treated with 50 mg of acid. -1The characteristic peak of the water of crystallization was stronger than that of the other groups, indicating that PVA may have interacted with attapulgite through hydrogen bonds. This proves that acid treatment is more conducive to the compounding of PVA, and 50 mg of acid treatment is the most suitable.
[0033] The infrared spectra of alkali-treated attapulgite / PVA are as follows: Figure 3 As shown in the figure, the order from 25mg alkali to 3010 coated paper (as indicated by the top-to-bottom arrangement on the drawing) corresponds to the order on the drawing. The figure shows that at 3264.66cm... -1 1085.62cm -1 834.72cm -1 472.12cm -1 The same characteristic peak exists in each group. And at 3264.66 cm⁻¹ -1 The characteristic peak for the stretching vibration of the hydroxyl group is 1085.62 cm⁻¹. -1 This is a strong absorption peak of the silicon-oxygen-silicon bond, which is the most typical and important characteristic of the silicon-oxygen-silicon bond. 834.72 cm⁻¹ -1 It is a Si-O-Si symmetrical bending vibration peak, 472.12 cm⁻¹. -1 These are Si-O-Si bending vibration peaks. The appearance of these three characteristic peaks proves the existence of silicon-oxygen-silicon bonds. Therefore, it can be seen that after PVA is modified with attapulgite, silicon-oxygen-silicon bonds successfully replace the hydroxyl groups on the surface. As shown in the figure, the characteristic peaks of attapulgite / PVA treated with different amounts of alkali differ, with a peak at 3264.66 cm⁻¹. -1 The characteristic peak of the hydroxyl group at 1085.62 cm⁻¹ -1 The strong absorption peak of the silicon-oxygen-silicon bond at 834.72 cm⁻¹ -1 The Si-O-Si symmetrical bending vibration peak at 472.12 cm⁻¹ -1 The intensity of the Si-O-Si bending vibration peaks decreased at all sites except for those treated with 150 mg alkali on attapulgite / PVA. Therefore, alkali treatment may be detrimental to the composite with PVA, and 150 mg alkali treatment is the most suitable.
[0034] The pH values of the acid / alkali treated attapulgite-modified PVA coating solution are shown in the table below.
[0035] As shown in the table above, with the increase of acid-treated attapulgite, more acid is adsorbed on the attapulgite, and the pH value of the acid-treated attapulgite-modified PVA coating solution is lower; with the increase of alkali-treated attapulgite, more alkali is adsorbed on the attapulgite, and the pH value of the alkali-treated attapulgite-modified PVA coating solution is higher.
[0036] like Figure 4The figure shows the tensile strength of acid-treated attapulgite-modified PVA barrier paper. The figure shows that the tensile strength of the base paper is 20.416 N·m / g. After coating with the coating solution, the tensile strength of each group of barrier papers was improved to varying degrees. This is because the film-forming properties of PVA enhance the mechanical properties of the base paper. After coating with the PVA coating solution, the tensile strength of the barrier paper reached 20.956 N·m / g, an increase of 2.64% compared to the base paper. With the increase of acid-treated attapulgite in PVA, the tensile strength of the acid-treated attapulgite / PVA barrier paper showed a trend of first increasing and then decreasing. When 50 mg of acid-treated attapulgite was added and blended with PVA, the acid-treated attapulgite / PVA barrier paper exhibited the highest tensile strength of 21.885 N·m / g, which was 7.2% higher than that of the base paper and also higher than the tensile strength of the 3010 coated paper series (21.469 N·m / g).
[0037] like Figure 5 As shown, the tensile strength of alkali-treated attapulgite-modified PVA is as follows: with the increase of alkali-treated attapulgite in PVA, the tensile strength of the alkali-treated attapulgite / PVA barrier paper first increases and then decreases. When 100 mg of alkali-treated attapulgite is added and blended with PVA, the tensile strength of the alkali-treated attapulgite / PVA barrier paper is the highest, at 22.827 N·m / g, which is 11.81% higher than that of the base paper, and its tensile strength is stronger than that of 3010 coated paper. With further increases in the amount added, the tensile strength of the barrier paper decreases.
[0038] The grease resistance of each group of barrier papers is shown in the table below. As can be seen from the figure, the grease resistance of acid / alkali treated attapulgite modified PVA barrier paper has been improved to varying degrees compared with the original paper, and the grease resistance grade of 50mg acid treated attapulgite modified PVA barrier paper is the highest grade 7. The reasons for the enhanced grease resistance are as follows: (1) Attapulgite can enhance the hydrophobicity of PVA, making it difficult for the paper surface to penetrate and absorb grease, thus improving its grease resistance; (2) Attapulgite can fill and seal some of the micropores in the PVA barrier paper, enhancing the isolation effect of PVA, making it more difficult for grease to penetrate into the paper interior, thus improving grease resistance; (3) Attapulgite can make the surface of PVA barrier paper rougher and looser, increasing the surface tension, reducing the contact area between the paper and grease, making it less likely to adhere to the surface, thus improving grease resistance. (4) Attapulgite can have a strong interfacial interaction with PVA, which makes the fiber and attapulgite particles tightly bonded together to form a composite structure that is not easily penetrated and damaged by grease, thus improving the oil resistance; (5) The addition of attapulgite can shield some of the hydroxyl groups in the paper, reduce the interaction with grease, and improve the grease resistance.
[0039]
[0040] Water phase contact angles of different barrier papers, such as Figure 6 and 7 As shown, the water phase contact angle of the base paper is 110.2°, while the water phase contact angle of the PVA barrier paper is smaller than that of the base paper. This is because PVA contains many hydroxyl groups, which can interact strongly with water molecules and exhibit strong hydrophilicity. The aqueous phase contact angle of attapulgite-modified PVA barrier paper treated with alkali is larger than that of acid-treated attapulgite-modified PVA barrier paper. When 100mg of alkali is used to treat attapulgite-modified PVA barrier paper, the aqueous phase contact angle is the largest at 92.4°. The reasons are as follows: (1) Alkali treatment will eliminate the siloxane groups on the surface of attapulgite to a certain extent, reducing hydrophilicity and weakening the interaction with water; (2) Under alkaline conditions, some hydroxyl groups undergo dehydration reaction to generate ester bonds or ether bonds, resulting in a certain degree of hydrophobic modification; (3) The interfacial interaction between attapulgite and PVA will be affected by alkali treatment, and the interfacial bonding force between attapulgite and PVA will be weakened, making it difficult to form a continuous capillary structure. This is also not conducive to the expansion of water inside the material, thus increasing the contact angle; (4) Alkali treatment will increase the density of the barrier paper surface, reduce the roughness, and decrease the bonding area with water.
[0041] Figure 8 The figure shows the oil phase contact angle test results for different barrier papers. As can be seen, the oil phase contact angle of the base paper is 87.3°, while the PVA barrier paper has a larger oil phase contact angle than the base paper. This is because PVA contains a large number of hydroxyl groups, and the interaction between hydroxyl groups and oil molecules is relatively weak. The acid-treated attapulgite-modified PVA barrier paper has a larger oil phase contact angle than the alkali-treated attapulgite-modified PVA barrier paper. The maximum oil phase contact angle is 92.6° when treated with 50mg of alkali. The increase in the oil phase contact angle of the attapulgite-modified PVA barrier paper due to acid treatment is mainly due to the changes in the attapulgite and PVA network under acid conditions. Acid treatment reduces the oleophilicity of attapulgite and PVA, makes the network structure denser, weakens the capillary effect, and causes changes in surface structure and energy that are unfavorable to wetting. The effect of hydrophobic groups is also suppressed. These changes collectively reduce the affinity between the material and oils, resulting in a larger oil phase contact angle compared to alkali treatment.
[0042] As shown in Figure 9, the base paper has the highest air permeability, allowing air to pass through most easily due to its loose fiber structure. After PVA coating, the air permeability of the paper decreased by 55.70%, which is caused by the combined effects of PVA itself on sealing, densification, capillary disruption, and changes in surface structure. The air permeability of the barrier paper initially decreased and then increased with increasing acid-treated attapulgite, with the lowest air permeability (1.27531 μm / Pa·s) observed in PVA barrier paper modified with 50 mg acid-treated attapulgite, even lower than that of 3010 coated paper. This represents a 59.30% decrease compared to the base paper and an 8.15% decrease compared to PVA barrier paper. When the acid-treated attapulgite exceeds 50 mg, excessive acid-treated attapulgite can, to some extent, damage the integrity of the PVA network, weakening the inhibitory effect of PVA on gas permeation and increasing air permeability.
[0043] As shown in Figure 10, with the increase of alkali-treated attapulgite, the air permeability of the barrier paper first decreased and then increased. The PVA barrier paper modified with 100 mg alkali-treated attapulgite exhibited the lowest air permeability at 1.3027 μm / Pa·s, which was even lower than that of 3010 coated paper. This represents a decrease of 58.43% compared to the base paper and a decrease of 6.17% compared to the PVA barrier paper. When the alkali-treated attapulgite content exceeded 100 mg, the large amount of alkali-treated attapulgite disrupted the PVA network, improved the surface structure, enhanced the effect of the attapulgite-PVA interface, and increased the air permeability.
[0044] As shown below, the PVA barrier paper modified with attapulgite using 50mg of acid treatment exhibits the lowest Cobb value and the best oil-resistant performance. This is mainly due to the combined oil-resistant and sealing effects of PVA and attapulgite. Simultaneously, the acid treatment conditions strengthen the bond between the two, altering the material's surface structure and energy, weakening the capillary effect, and shielding some lipophilic groups. These changes collectively improve the material's oil-blocking effect, resulting in a lower Cobb value compared to ordinary paper.
[0045]
[0046] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the claimed invention.
Claims
1. A composite coating liquid based on attapulgite modification, characterized in that, This includes modifying attapulgite and then heating and mixing it with an aqueous solution of polyvinyl alcohol to obtain a composite coating liquid. When this composite coating liquid is applied to paper, the air permeability is adjusted to 1.27531 μm / Pa·s. The preparation method of the composite coating liquid based on attapulgite modification includes the following steps: S1. First, take a sample of the modified solution, then add attapulgite to mix, and obtain solution A. The modified solution is a 5 mol / L dilute hydrochloric acid solution. S2. Centrifuge the obtained solution A to separate the dilute hydrochloric acid from the surface of the attapulgite, then wash, dehydrate and dry to obtain modified attapulgite. When centrifuging solution A, use a high speed of 9500 r / min for at least 2 min. S3. Subsequently, the modified attapulgite is placed in a polyvinyl alcohol aqueous solution and heated and stirred in water at a constant temperature of 90°C to obtain a composite coating liquid.
2. The composite coating liquid based on attapulgite modification according to claim 1, characterized in that, In step S1, after adding attapulgite, the mixing is carried out under stirring conditions for 6 hours to allow the modified liquid to fully contact and react with the surface of the attapulgite.
3. The composite coating liquid based on attapulgite modification according to claim 1, characterized in that, The ratio of polyvinyl alcohol to water in the S3 aqueous solution is 5g PVA / 95mL water.
4. The composite coating liquid based on attapulgite modification according to claim 1, characterized in that, In step S3, when the mixture is heated and stirred in water at a constant temperature of 90°C, a water bath heating method is used.
5. The composite coating liquid based on attapulgite modification according to claim 1, characterized in that, Application of the composite coating liquid: The obtained composite coating liquid is coated on the surface of paper to form barrier paper, which is then dried to remove solvent and moisture, thereby obtaining modified attapulgite / PVA barrier paper.
Citation Information
Patent Citations
Attapulgite-containing water-based paint for cigarette wrap paper
CN101914870B
Polyvinyl alcohol / attapulgite clay nano-composite film and its preparation method
CN102432967A
Preparation method of hydrophobic oilproof paper
CN108625219A